A composite collector for flotation of nonferrous metal sulfide ores and its preparation method and application
By preparing a composite collector containing ethoxycarbonylhexylthiourea, benzoylthiourea and ethoxycarbonylbutylthiourea, the problem of insufficient collection power and selectivity in the separation of multi-metallic complex sulfide ores is solved. It achieves efficient separation of copper-zinc, copper-sulfur, copper-cobalt and other metals and reduces the arsenic content in copper concentrate, and is suitable for the flotation process of various sulfide ores.
Patent Information
- Application Number
- CN202211653016.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-22
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-12-22
AI Technical Summary
Existing technologies have problems with insufficient collection power and selectivity in the separation of polymetallic complex sulfide ores, making it difficult to achieve efficient separation of target metals.
A composite collector is used, including ethoxycarbonylhexylthiourea, benzoylthiourea, ethoxycarbonylbutylthiourea and solvent oil, which is prepared through a specific ratio and stirring process to form a floating collector. The yellow transparent liquid collector is suitable for efficient separation of copper zinc, copper sulfur, copper cobalt and other metals.
This collector shows strong collection power and selectivity in the separation of copper-zinc, copper-sulfur, copper-cobalt and other metals, can significantly reduce the arsenic content in copper concentrate, and works stably under low pH conditions, reducing The dosage of reagent is suitable for the flotation process of various sulfide ores.
Smart Images

Figure CN115739399B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of mineral processing, and relates to a composite collector for floating nonferrous metal sulfide ores, and a preparation method and application thereof. Background Art
[0002] Traditional collectors for non-ferrous metal sulfide ores include xanthate, black medicine, ethiocarbamate (Z-200), etc. Xanthate and black medicine have strong collecting power, but poor selectivity. The separation index in the multi-metal flotation separation process is not very ideal. They usually need to be used together with inhibitors or other regulators, especially for some "poor, mixed, and difficult to select" ores. Therefore, the development of new sulfide ore collectors with strong collecting power and good selectivity has a good market application prospect, especially the composite collectors with synergistic effects are more advantageous.
[0003] At present, many composite collectors for sulfide ores have been developed and put into popularization and application. Patent CN 103464292A introduces a sulfide and oxidized mixed copper ore dressing agent, which is made of oleic acid, sodium carbonate, sodium silicate, styrenephosphonic acid, hydroxybutyl vinyl ether, quicklime, and activator. The collector has the characteristics of high separation efficiency, high yield, low reagent cost, small dosage, simple and reliable process flow, easy operation, low investment, and low dressing cost, and is suitable for the dressing of composite sulfide and oxidized mixed copper ores. Patent CN 104826742A provides a composite collector for sulfide ores and a preparation method thereof, comprising: 10-15% dialkyl monothiophosphate, 15-30% alkyl monothioformate, 15-40% dialkyl dithiophosphate, 5-15% cosolvent, 13-15% dialkyl thiocarbamate, and 10-20% water. The invention has the advantages of small dosage, low cost, and convenient reagent addition, and has good recovery indicators for metal copper, gold, silver, etc., has a composite effect, collecting property and foaming property in the flotation process, and has good selectivity and excellent collecting effect on useful metals in mud-containing minerals. In practical applications, it can also comprehensively recover useful metal minerals from complex minerals. Patent CN 107252735A provides a composite collector for flotation of sulfur ore, and a preparation method and application thereof. The composite collector is composed of X oil and hydrocarbon oil. The preparation method is to use hydrocarbon oil as a solvent, react X oil with phosphorus pentasulfide, and obtain a composite collector composed of modified X oil and hydrocarbon oil. The agent has strong collecting ability and selectivity for sulfide ores such as copper sulfide, copper-molybdenum ore, lead-zinc ore, etc., and obtains good flotation indicators in flotation tests. CN 107138287 A provides a preparation method and use of a combined collector for flotation of sulfide ore, wherein the combined collector is composed of 7-13 parts of butoxycarbonyl isobutyl thiocarbamate, 30-50 parts of butoxycarbonyl hexyl thiocarbamate, 2-10 parts of 2-ethylhexanol, 3-6 parts of butanol, 15-40 parts of a fatty alcohol mixture, 5-10 parts of hydrocarbons, 3-6 parts of butanol, 0.1-1 parts of quinoline, and 0.5-1.25 parts of substituted acrolein. The collector improves the recovery rate of mineral processing while maintaining good selectivity, and can reduce the arsenic content in the concentrate. Patent CN 99122607 introduces a composite reagent composed of alkyl ammonium dithiophosphate, alkyl thiocarbamate, C6-C8 mixed alcohol and water. The reagent is suitable for non-ferrous metals and precious metals such as copper, lead, nickel, gold and silver, and can improve the metal recovery rate and concentrate grade, and reduce the content of impurities in the concentrate product.Patent CN 10199215A introduces a high-sulfur copper ore collector, the material composition: 40-50 parts of alkyl allyl thiocarbamate, 35-45 parts of thiocyanate, 8-15 parts of alkyl xanthate cyanate, the collector has the dual properties of collecting and foaming, good selectivity, strong collecting ability, and can achieve efficient separation of copper and sulfur in the pH range of 7-10, which can effectively improve the concentrate grade and recovery rate. It is a high-sulfur copper ore collector with a wide range of applications; Patent CN 1411910A introduces a flotation sulfide ore collector with good selectivity and strong collecting ability, which is mainly prepared by thiocarbamate, diethylthiocyanate, 730A, dialkyl dithiophosphate, and butanesulfonic acid propylene ester in proportion. It can significantly improve the mineral processing technical indicators, effectively separate copper sulfur, copper iron, copper arsenic, etc., and reduce the loss of valuable elements. Although the patented composite reagents introduced above have their own characteristics, they have certain flotation effects on sulfide ores or mixed ores, and have relatively good capture and selectivity for specific ores, but they have some limitations in the separation of multi-metal complex sulfide ores, and cannot perform efficient separation of target metals. Therefore, it is of great significance to develop new and efficient composite reagents for non-ferrous metal sulfide ores. Summary of the invention
[0004] In order to improve the flotation separation index of metals, the present invention provides a composite collector for flotation of non-ferrous metal sulfide ores, a preparation method and application thereof. The composite collector has excellent application effect in the flotation process of non-ferrous metal ores containing copper, molybdenum, lead, cobalt, arsenic, gold, silver and the like, can achieve efficient separation of copper-zinc, copper-sulfur and copper-cobalt, and can significantly reduce the arsenic content in copper concentrate.
[0005] The invention provides a composite collector for flotation of nonferrous metal sulfide ores, comprising the following components: ethoxycarbonyl hexyl thiocarbamate, benzoyl thiocarbamate, ethoxycarbonyl butyl thiourea, solvent oil and fusel alcohol.
[0006] Composite collector for flotation of nonferrous metal sulfide ores, each component is calculated by weight:
[0007] 20-40 parts of ethoxycarbonyl hexyl thiocarbamate, 10-40 parts of benzoyl thiocarbamate, 10-30 parts of ethoxycarbonyl butyl thiourea, 5-20 parts of fusel alcohol, and 5-20 parts of solvent naphtha.
[0008] Furthermore, the purity of the ethoxycarbonyl hexylthiocarbamate is>90%, the purity of the benzoyl isobutylthiocarbamate is>80%, and the purity of the ethoxycarbonyl butylthiourea is>90%.
[0009] Furthermore, the solvent oil is an industrial raw material, one or more combinations of No. 70, No. 90, No. 120, No. 180, No. 190, No. 200, No. 260 and fuel solvents such as gasoline, kerosene, and diesel, preferably No. 120 solvent oil.
[0010] Furthermore, the alcohol is at least two of C4-C12 fatty alcohols, preferably a mixture of isobutyl alcohol and methyl isobutyl carbinol.
[0011] Furthermore, the mixture of isobutanol and methyl isobutyl carbinol comprises 10 to 30 parts of isobutanol and 70 to 90 parts of methyl isobutyl carbinol; preferably, 15 parts of isobutanol and 85 parts of methyl isobutyl carbinol.
[0012] Furthermore, the preparation method of the mixture of isobutyl alcohol and methyl isobutyl carbinol is as follows: the ingredients are prepared according to the above raw material ratio, and the mixture is stirred and mixed in a mixing container for 30 minutes to obtain the mixture.
[0013] The preparation method of the composite collector for flotation of non-ferrous metal sulfide ores specifically comprises the following steps:
[0014] The ingredients are prepared according to the mass fractions of the raw materials of the above composite collector. At room temperature and under stirring conditions, ethoxycarbonyl hexyl thiocarbamate, benzoyl thiocarbamate, fusel alcohol and solvent oil are added to the mixing tank in sequence. The mixture is stirred for 30 minutes at a stirring speed of 130 r / min. After the materials are evenly mixed and transparent, ethoxycarbonyl butyl thiourea is added and stirred for 60 minutes. After the materials are evenly mixed and transparent, the composite collector for flotation of non-ferrous metal sulfide ores of the present invention can be obtained. The product is a yellow transparent liquid with a slightly special odor.
[0015] The composite collector of the present invention is mainly used in sulfide ore flotation processes such as copper-zinc separation, lead-zinc separation, copper-cobalt separation, and copper, molybdenum, gold and silver recovery.
[0016] Compared with the prior art, the beneficial effects of the present invention are as follows.
[0017] 1. Strong collecting power: The composite collector of the present invention has strong collecting power for copper, lead, gold and silver in various non-ferrous metal sulfide ores, and has a high recovery rate.
[0018] 2. Good selectivity: The composite collector of the present invention has weaker capture power for unactivated zinc, cobalt and pyrite in various non-ferrous metal sulfide ores, and the grade in the concentrate is higher.
[0019] 3. Foaming property: The composite collector of the present invention has certain foaming property, and in practical application, no foaming agent or less foaming agent may be added.
[0020] 4. Small dosage: Due to the strong collector and good selectivity, the composite collector of the present invention has a smaller dosage in practical applications than traditional yellow medicine, black medicine, ethiocarbamate and other agents, usually 1 / 3-2 / 3 of their dosage.
[0021] 5. Applicable under low pH conditions: The composite collector of the present invention is stable under low pH conditions and can function under acidic or weakly alkaline conditions, which is beneficial to the recovery of valuable metals and can improve the problem of low recovery rate of associated metals such as gold and silver under high pH conditions.
[0022] 6. Adjustability: For different sulfide ores, the components of the composite collector can be adjusted within a certain range according to the selection index data in the actual process. Combined with the appropriate reagent system, the comprehensive flotation index can be improved. Therefore, this reagent has a wider range of applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 Example 1 Flow chart of pharmaceutical test.
[0024] Figure 2 Example 2 Flow chart of pharmaceutical test. DETAILED DESCRIPTION
[0025] The present invention is further described below in conjunction with specific implementation methods, but the scope of protection required is not limited to the description.
[0026] The present invention provides a composite collector for flotation of non-ferrous metal sulfide ores, comprising the following components in parts by mass: 20 to 40 parts of ethoxycarbonyl hexyl thiocarbamate, 10 to 40 parts of benzoyl thiocarbamate, 10 to 30 parts of ethoxycarbonyl butyl thiourea, 5 to 20 parts of solvent oil, and 5 to 20 parts of fusel alcohol.
[0027] Furthermore, the purity of the ethoxycarbonyl hexylthiocarbamate is>90%, the purity of the benzoyl isobutylthiocarbamate is>80%, and the purity of the ethoxycarbonyl butylthiourea is>90%.
[0028] Furthermore, the solvent oil is an industrial raw material, one or more combinations of No. 70, No. 90, No. 120, No. 180, No. 190, No. 200, No. 260 and fuel solvents such as gasoline, kerosene, and diesel, preferably No. 120 solvent oil.
[0029] Furthermore, the alcohol is at least two of C4-C12 fatty alcohols, preferably a mixture of isobutyl alcohol and methyl isobutyl carbinol.
[0030] Furthermore, the mixture of isobutanol and methyl isobutyl carbinol comprises 10 to 30 parts of isobutanol and 70 to 90 parts of methyl isobutyl carbinol; preferably, 15 parts of isobutanol and 85 parts of methyl isobutyl carbinol.
[0031] Furthermore, the preparation method of the mixture of isobutyl alcohol and methyl isobutyl carbinol is as follows: the ingredients are prepared according to the above raw material ratio, and the mixture is stirred and mixed in a mixing container for 30 minutes to obtain the mixture.
[0032] The preparation method of the composite collector for flotation of non-ferrous metal sulfide ores specifically comprises the following steps:
[0033] The ingredients are prepared according to the mass fractions of the raw materials of the above composite collector. At room temperature and under stirring conditions, ethoxycarbonyl hexyl thiocarbamate, benzoyl thiocarbamate, fusel alcohol and solvent oil are added to the mixing tank in sequence. The mixture is stirred for 30 minutes at a stirring speed of 130 r / min. After the materials are evenly mixed and transparent, ethoxycarbonyl butyl thiourea is added and stirred for 60 minutes. After the materials are evenly mixed and transparent, the composite collector for flotation of non-ferrous metal sulfide ores of the present invention can be obtained. The product is a yellow transparent liquid with a slightly special odor.
[0034] The composite collector of the present invention is mainly used in sulfide ore flotation processes such as copper-zinc separation, lead-zinc separation, copper-cobalt separation, and copper, molybdenum, gold and silver recovery.
[0035] Example 1.
[0036] The mass proportions of the composite pharmaceutical components are as follows: 20 parts of ethoxycarbonyl hexyl thiocarbamate, 40 parts of benzoyl thiocarbamate, 20 parts of ethoxycarbonyl butyl thiourea, 15 parts of fusel alcohol (the mass ratio of isobutyl alcohol to methyl isobutyl carbinol is 15:85), and 5 parts of No. 120 solvent oil.
[0037] The preparation method of the composite collector specifically comprises the following steps:
[0038] The ingredients are prepared according to the mass fractions of the raw materials of the above composite collector. At room temperature and under stirring conditions, ethoxycarbonyl hexyl thiocarbamate, benzoyl thiocarbamate, fusel alcohol and solvent oil are added to the mixing tank in sequence. The mixture is stirred for 30 minutes at a stirring speed of 130 r / min. After the materials are evenly mixed and transparent, ethoxycarbonyl butyl thiourea is added and stirred for 60 minutes. After the materials are evenly mixed and transparent, the composite collector for flotation of non-ferrous metal sulfide ores of the present invention can be obtained.
[0039] The main metal minerals in the ore used for verification are chalcopyrite, sphalerite, pyrite and pyrrhotite, in addition, there are small amounts of magnetite and galena, etc. There are many types of gangue minerals, mainly quartz, feldspar, tremolite, biotite, followed by muscovite, sericite, diopside, chlorite and small amounts of wollastonite, garnet, apatite, carbonate minerals, sillimanite, etc. The preferential copper flotation process is adopted to achieve copper and zinc separation and produce copper concentrate.
[0040] Based on the slurry pH value and adjusting agent test, the reagent test uses the composite collector of the present invention and butyl yellow and ethyl thiocarbamate, which have good collection effects on copper minerals, to conduct comparative tests. Figure 1 , the test results are shown in Table 1.
[0041] Table 1 Results of drug comparison test (%).
[0042]
[0043] From the test results in Table 1, it can be seen that the composite collector of the present invention has good capture performance for copper sulfide, and its capture power is better than that of ethylthiocarbamate, and its selectivity is better than that of butyl yellow.
[0044] Example 2.
[0045] The mass proportions of the composite pharmaceutical components are as follows: 40 parts of ethoxycarbonyl hexyl thiocarbamate, 10 parts of benzoyl thiocarbamate, 30 parts of ethoxycarbonyl butyl thiourea, 15 parts of fusel alcohol (the mass ratio of isobutyl alcohol to methyl isobutyl carbinol is 15:85), and 5 parts of No. 120 solvent oil.
[0046] The preparation method of the composite collector specifically comprises the following steps:
[0047] The ingredients are prepared according to the mass fractions of the raw materials of the above composite collector. At room temperature and under stirring conditions, ethoxycarbonyl hexyl thiocarbamate, benzoyl thiocarbamate, fusel alcohol and solvent oil are added to the mixing tank in sequence. The mixture is stirred for 30 minutes at a stirring speed of 130 r / min. After the materials are evenly mixed and transparent, ethoxycarbonyl butyl thiourea is added and stirred for 60 minutes. After the materials are evenly mixed and transparent, the composite collector for flotation of non-ferrous metal sulfide ores of the present invention can be obtained.
[0048] The ores used for verification mainly contain two valuable metals, copper and molybdenum, and the others are pyrite, galena, sphalerite, and the metal oxides are mainly magnetite, etc. The gangue minerals are mainly quartz, muscovite, a small amount of feldspar, illite, kaolin, zircon, rutile, etc. See the test process for details. Figure 2 , the test results are shown in Table 2.
[0049] Table 2 Results of drug comparison test (%).
[0050]
[0051] It can be seen from the test results in Table 2 that the composite collector of the present invention has good collecting power and selectivity for copper-molybdenum minerals.
[0052] Example 3.
[0053] The mass proportions of the composite pharmaceutical components are as follows: 40 parts of ethoxycarbonyl hexyl thiocarbamate, 30 parts of benzoyl thiocarbamate, 10 parts of ethoxycarbonyl butyl thiourea, 15 parts of fusel alcohol (the mass ratio of isobutyl alcohol to methyl isobutyl carbinol is 15:85), and 5 parts of No. 120 solvent oil.
[0054] The preparation method of the composite collector specifically comprises the following steps:
[0055] The ingredients are prepared according to the mass fractions of the raw materials of the above composite collector. At room temperature and under stirring conditions, ethoxycarbonyl hexyl thiocarbamate, benzoyl thiocarbamate, fusel alcohol and solvent oil are added to the mixing tank in sequence. The mixture is stirred for 30 minutes at a stirring speed of 130 r / min. After the materials are evenly mixed and transparent, ethoxycarbonyl butyl thiourea is added and stirred for 60 minutes. After the materials are evenly mixed and transparent, the composite collector for flotation of non-ferrous metal sulfide ores of the present invention can be obtained.
[0056] The ores used for verification mainly include chalcopyrite, bornite, blue chalcocite, covellite, arsenopyrite, silver chalcopyrite, argentite, pyrite, and the gangue minerals are mainly quartz, feldspar, sericite, carbonate minerals, etc. The test results are shown in Table 3.
[0057] Table 3 Results of drug comparison test (%).
[0058]
[0059] It can be seen from the test results in Table 3 that the composite collector of the present invention has a strong ability to capture copper and a good selectivity for arsenic, and can significantly reduce the arsenic content in the copper concentrate.
Claims
1. A composite collector for flotation of non-ferrous metal sulfide ores, characterized in that: The invention comprises the following components in parts by weight: 20 to 40 parts of ethoxycarbonyl hexyl thiocarbamate, 10 to 40 parts of benzoyl thiocarbamate, 10 to 30 parts of ethoxycarbonyl butyl thiourea, 5 to 20 parts of solvent oil and 5 to 20 parts of fusel alcohol.
2. The composite collector for flotation of non-ferrous metal sulfide ores according to claim 1, characterized in that: 20 parts of ethoxycarbonyl hexyl thiocarbamate, 40 parts of benzoyl thiocarbamate, 20 parts of ethoxycarbonyl butyl thiourea, 15 parts of fusel alcohol, and 5 parts of solvent oil.
3. The composite collector for flotation of nonferrous metal sulfide ores according to claim 1, characterized in that: 40 parts of ethoxycarbonyl hexyl thiocarbamate, 10 parts of benzoyl thiocarbamate, 30 parts of ethoxycarbonyl butyl thiourea, 15 parts of fusel alcohol, and 5 parts of solvent oil.
4. The composite collector for flotation of nonferrous metal sulfide ores according to claim 1, characterized in that: 40 parts of ethoxycarbonyl hexyl thiocarbamate, 30 parts of benzoyl thiocarbamate, 10 parts of ethoxycarbonyl butyl thiourea, 15 parts of fusel alcohol, and 5 parts of solvent oil.
5. The composite collector for flotation of non-ferrous metal sulfide ores according to any one of claims 1 to 4, characterized in that: The purity of the ethoxycarbonyl hexylthiocarbamate is greater than 90%, the purity of the benzoyl isobutylthiocarbamate is greater than 80%, and the purity of the ethoxycarbonyl butylthiourea is greater than 90%.
6. The composite collector for flotation of nonferrous metal sulfide ores according to any one of claims 1 to 4, characterized in that: The solvent oil is an industrial raw material, one or more combinations of No. 70, No. 90, No. 120, No. 180, No. 190, No. 200, and No. 260 fuel solvents.
7. The composite collector for flotation of non-ferrous metal sulfide ores according to any one of claims 1 to 4, characterized in that: The alcohol is C4-C 12 At least two of the fatty alcohols.
8. The composite collector for flotation of non-ferrous metal sulfide ores according to any one of claims 1 to 4, characterized in that: The fusel alcohol is a mixture of isobutyl alcohol and methyl isobutyl carbinol, wherein the isobutyl alcohol comprises 10 to 30 parts and the methyl isobutyl carbinol comprises 70 to 90 parts; the mixture is stirred and mixed in a mixing container for 30 minutes to obtain the mixture.
9. A method for preparing a composite collector for flotation of non-ferrous metal sulfide ores, characterized in that: The specific steps include: The raw materials of the composite collector according to any one of claims 2 to 4 are prepared in the following proportions by mass: ethoxycarbonyl hexylthiocarbamate, benzoylthiocarbamate, fusel alcohol and solvent oil are sequentially added to a mixing tank at room temperature and under stirring conditions; the mixture is stirred for 30 minutes at a stirring speed of 130 r / min; after the materials are uniformly mixed and transparent, ethoxycarbonyl butylthiourea is added and stirred for 60 minutes; after the materials are uniformly mixed and transparent, the composite collector for flotation of non-ferrous metal sulfide ores can be obtained.