Preparation method of high-purity nickel carbonate
By using the reaction of soluble nickel salt and ammonium bicarbonate, combined with the auxiliary effect of ammonium oleate, high-purity nickel carbonate was successfully prepared, solving the purity and particle size of nickel carbonate in the prior art, and improving the performance of lithium-ion battery materials and environmentally friendly.
Patent Information
- Application Number
- CN202411137863.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-19
AI Technical Summary
The prior art is difficult to prepare high-purity nickel carbonate, resulting in high impurity content in lithium-ion battery materials, affecting the stability and performance of the battery, and serious pollution in the impurity removal process, increasing the difficulty of wastewater treatment.
Using soluble nickel salt and ammonium bicarbonate as the main reaction raw material, adding ammonium oleate as the auxiliary agent, and by stirring evenly, heating reaction, centrifugation separation, washing and drying, high-purity nickel carbonate, ammonium oleate as the Emulsifier improves the dispersion of the reaction liquid, and decomposes insoluble oleic acid at high temperatures, coats nickel carbonate to avoid invasion of impurities and improves purity.
The high purity preparation of nickel carbonate was achieved, with a purity of more than 99.6%, a particle size was reduced, which improved the stability and electrochemical properties of the battery material, reduced environmental pollution, and simplified wastewater treatment.
Smart Images

Figure CN118978195A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of nickel carbonate, and in particular to a method for preparing high-purity nickel carbonate. Background Art
[0002] At present, nickel carbonate is an important basic chemical raw material. Ordinary industrial-grade nickel carbonate products or solutions can meet the needs of fertilizers, coatings, catalysts, ceramics, mineral processing and other fields, but cannot meet the use requirements in the field of lithium-ion battery materials. Lithium manganese oxide materials and nickel-cobalt-manganese multi-element materials have very high requirements for the purity of nickel carbonate. Lithium manganese oxide and nickel-cobalt-manganese multi-element materials are the core direction of the demand for lithium-ion battery materials. With the gradual promotion and application of lithium-ion batteries in new energy vehicles, the demand for high-purity nickel carbonate will explode. Therefore, the preparation and production technology of high-purity nickel carbonate has become a research hotspot in the field of manganese metallurgy.
[0003] In recent years, the number of lithium-ion batteries used has increased exponentially. Nickel-containing raw materials, such as nickel ore and other recycled raw materials, are doped with a large amount of other impurities, such as calcium, magnesium, zinc, copper, etc., so impurities must be removed during the preparation process. The purity requirement for battery-grade nickel carbonate is relatively high, generally reaching more than 99.98%. High-purity nickel carbonate can ensure the stability, conductivity and electrochemical properties of electrode materials, improve the service life and energy storage density of batteries, and is therefore widely used in battery manufacturing. However, the impurity content in battery-grade nickel carbonate prepared using existing processes is relatively high. Even if it meets the standards, fluorides or sulfides are used for impurity removal, which not only causes environmental pollution, but also increases the difficulty of wastewater treatment. Therefore, it is urgent to design a new method for preparing high-purity nickel carbonate. Summary of the invention
[0004] In view of the problems existing in the prior art, the object of the present invention is to provide a method for preparing high-purity nickel carbonate.
[0005] The purpose of the present invention is achieved by adopting the following technical solutions:
[0006] A method for preparing high-purity nickel carbonate comprises the following steps:
[0007] Step 1, mixing a soluble nickel salt into deionized water, and stirring thoroughly until the nickel salt is uniformly dissolved to obtain a first mixed solution;
[0008] Step 2, mixing ammonium bicarbonate, ammonium oleate and deionized water, and stirring them thoroughly to obtain a second mixed solution;
[0009] Step 3, adding the second mixed liquid dropwise into the first mixed liquid to obtain a third mixed liquid;
[0010] Step 4, pouring the third mixed liquid into a reactor, heating it, and after the reaction is completed, centrifuging and collecting the solid to obtain a crude product;
[0011] Step 5, washing and drying the crude product in sequence to obtain high-purity nickel carbonate.
[0012] Preferably, in step 1, the soluble nickel salt is a mixture of one or more of nickel sulfate, nickel nitrate and nickel chloride.
[0013] Preferably, in step 1, the mass volume ratio of the soluble nickel salt to deionized water is (0.15-0.3) g:(20-40) mL.
[0014] Preferably, in step 2, the mass volume ratio of ammonium bicarbonate, ammonium oleate and deionized water is (0.1-0.2) g: (0.5-1) g: (20-40) mL.
[0015] Preferably, in step 3, the volume ratio of the first mixed liquid to the second mixed liquid is 1:1.1-1.5.
[0016] Preferably, in step 3, after the dropwise addition is completed, stirring is continued for 10-20 min at a stirring speed of 100-200 r / min.
[0017] Preferably, in step 4, the reaction temperature is 150-200° C. and the reaction time is 6-12 h.
[0018] Preferably, in step 4, the centrifugal speed is 3000-5000 r / min.
[0019] Preferably, in step 5, washing is performed by washing three times with anhydrous ethanol and pure water in sequence, and drying is performed by vacuum drying at 40-60°C.
[0020] The beneficial effects of the present invention are:
[0021] 1. The present invention provides a method for synthesizing nickel carbonate, using soluble nickel salt and ammonium bicarbonate as reaction raw materials and ammonium oleate as an auxiliary enhancer, thereby reducing the particle size of the generated nickel carbonate and improving the purity of the nickel carbonate.
[0022] 2. In the synthesis process of nickel carbonate of the present invention, the reactant ammonium bicarbonate is easily decomposed, and the decomposition rate is faster when the temperature rises. However, too fast decomposition will reduce the reaction efficiency. The added ammonium oleate is weakly alkaline and can reduce the decomposition rate of ammonium bicarbonate to a certain extent.
[0023] 3. Ammonium oleate has two functions in the reaction process of the present invention. The first function is that it can be dissolved in water at low temperatures and can be used as an emulsifier to make the reaction solution more evenly dispersed, thereby reducing the particle size of the generated nickel carbonate. The second function is that it will gradually decompose into water-insoluble oleic acid at a higher temperature. Oleic acid has a strong capture property and can be coated on the surface of the generated nickel carbonate, thereby avoiding the invasion of water-soluble anions (such as sulfate, chloride, nitrate, etc.), thereby improving the purity of the product. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] The present invention is further described using the accompanying drawings, but the embodiments in the accompanying drawings do not constitute any limitation to the present invention. A person skilled in the art can obtain other drawings based on the following drawings without creative work.
[0025] Figure 1 It is a scanning electron microscope (SEM) schematic diagram of the nickel carbonate prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0026] The technical solution of the present invention is described below through specific examples. It should be understood that the one or more method steps mentioned in the present invention do not exclude the existence of other method steps before and after the combination step or the insertion of other method steps between these explicitly mentioned steps; it should also be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or to limit the scope of the present invention. The change or adjustment of the relative relationship thereof shall also be regarded as the scope of the present invention without substantially changing the technical content.
[0027] In order to better understand the above technical scheme, the exemplary embodiments of the present invention are described in more detail below. Although exemplary embodiments of the present invention are shown, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided in order to enable a more thorough understanding of the present invention and to enable the scope of the present invention to be fully communicated to those skilled in the art.
[0028] The present invention will be further described below in conjunction with the following examples.
[0029] Example 1
[0030] A method for preparing high-purity nickel carbonate comprises the following steps:
[0031] Step 1, mixing nickel sulfate into deionized water, the mass volume ratio of nickel sulfate to deionized water being 0.22 g:30 mL, and stirring thoroughly until the nickel sulfate is uniformly dissolved to obtain a first mixed solution;
[0032] Step 2, mixing ammonium bicarbonate, ammonium oleate and deionized water, wherein the mass volume ratio of ammonium bicarbonate, ammonium oleate and deionized water is 0.15 g:0.75 g:30 mL, and stirring well to obtain a second mixed solution;
[0033] Step 3, adding the second mixed liquid dropwise into the first mixed liquid, the volume ratio of the first mixed liquid to the second mixed liquid being 1:1.3, and after the dropwise addition, continuing stirring for 15 minutes at a stirring speed of 150 r / min to obtain a third mixed liquid;
[0034] Step 4, pouring the third mixed liquid into a reactor, placing the reactor at 180° C. for 9 hours, and after the reaction is completed, centrifuging to collect the solid at a centrifugal speed of 4000 r / min to obtain a crude product;
[0035] Step 5, washing the crude product three times with anhydrous ethanol and pure water in sequence, and vacuum drying at 50° C. for 10 h to obtain high-purity nickel carbonate.
[0036] Example 2
[0037] A method for preparing high-purity nickel carbonate comprises the following steps:
[0038] Step 1, mixing nickel nitrate into deionized water, the mass volume ratio of nickel nitrate to deionized water is 0.25g:25mL, and stirring until the nickel nitrate is uniformly dissolved to obtain a first mixed solution;
[0039] Step 2, mixing ammonium bicarbonate, ammonium oleate and deionized water, wherein the mass volume ratio of ammonium bicarbonate, ammonium oleate and deionized water is 0.12 g:0.6 g:30 mL, and stirring well to obtain a second mixed solution;
[0040] Step 3, adding the second mixed liquid dropwise into the first mixed liquid, the volume ratio of the first mixed liquid to the second mixed liquid is 1:1.2, and after the dropwise addition is completed, stirring is continued for 20 minutes at a stirring speed of 100 r / min to obtain a third mixed liquid;
[0041] Step 4, pouring the third mixed liquid into a reactor, placing the reactor at 160° C. for 10 hours, and after the reaction is completed, centrifuging to collect the solid at a centrifugal speed of 5000 r / min to obtain a crude product;
[0042] Step 5, washing the crude product three times with anhydrous ethanol and pure water in sequence, and vacuum drying at 40° C. for 12 h to obtain high-purity nickel carbonate.
[0043] Example 3
[0044] A method for preparing high-purity nickel carbonate comprises the following steps:
[0045] Step 1, mixing nickel chloride into deionized water, the mass volume ratio of nickel chloride to deionized water is 0.26g:30mL, and stirring until the mixture is uniformly dissolved to obtain a first mixed solution;
[0046] Step 2, mixing ammonium bicarbonate, ammonium oleate and deionized water, wherein the mass volume ratio of ammonium bicarbonate, ammonium oleate and deionized water is 0.17 g:0.8 g:30 mL, and stirring well to obtain a second mixed solution;
[0047] Step 3, adding the second mixed liquid dropwise into the first mixed liquid, the volume ratio of the first mixed liquid to the second mixed liquid being 1:1.4, and after the dropwise addition, continuing stirring for 15 minutes at a stirring speed of 100 r / min to obtain a third mixed liquid;
[0048] Step 4, pouring the third mixed liquid into a reactor, placing the reactor at 170° C. for 8 hours, and after the reaction is completed, centrifuging to collect the solid at a centrifugal speed of 4000 r / min to obtain a crude product;
[0049] Step 5, washing the crude product three times with anhydrous ethanol and pure water in sequence, and vacuum drying at 50° C. for 8 h to obtain high-purity nickel carbonate.
[0050] Example 4
[0051] A method for preparing high-purity nickel carbonate comprises the following steps:
[0052] Step 1, mixing nickel chloride into deionized water, the mass volume ratio of nickel chloride to deionized water is 0.15g:20mL, and stirring until it is evenly dissolved to obtain a first mixed solution;
[0053] Step 2, mixing ammonium bicarbonate, ammonium oleate and deionized water, wherein the mass volume ratio of ammonium bicarbonate, ammonium oleate and deionized water is 0.1 g:0.5 g:20 mL, and stirring well to obtain a second mixed solution;
[0054] Step 3, adding the second mixed liquid dropwise into the first mixed liquid, the volume ratio of the first mixed liquid to the second mixed liquid being 1:1.1, and after the dropwise addition, continuing stirring for 10 minutes at a stirring speed of 100 r / min to obtain a third mixed liquid;
[0055] Step 4, pouring the third mixed liquid into a reactor, placing the reactor at 150° C. for 6 hours, and after the reaction is completed, centrifuging to collect the solid at a centrifugal speed of 3000 r / min to obtain a crude product;
[0056] Step 5, washing the crude product with anhydrous ethanol and pure water three times in sequence, and vacuum drying at 40° C. for 10 h to obtain high-purity nickel carbonate.
[0057] Example 5
[0058] A method for preparing high-purity nickel carbonate comprises the following steps:
[0059] Step 1, mixing nickel sulfate into deionized water, the mass volume ratio of nickel sulfate to deionized water is 0.3g:40mL, and stirring until the nickel sulfate is uniformly dissolved to obtain a first mixed solution;
[0060] Step 2, mixing ammonium bicarbonate, ammonium oleate and deionized water, wherein the mass volume ratio of ammonium bicarbonate, ammonium oleate and deionized water is 0.2 g:1 g:40 mL, and stirring well to obtain a second mixed solution;
[0061] Step 3, adding the second mixed liquid dropwise into the first mixed liquid, the volume ratio of the first mixed liquid to the second mixed liquid being 1:1.5, and after the dropwise addition, continuing stirring for 20 minutes at a stirring speed of 200 r / min to obtain a third mixed liquid;
[0062] Step 4, pouring the third mixed liquid into a reactor, placing the reactor at 200° C. for 12 hours, and after the reaction is completed, centrifuging to collect the solid at a centrifugal speed of 5000 r / min to obtain a crude product;
[0063] Step 5, washing the crude product three times with anhydrous ethanol and pure water in sequence, and vacuum drying at 60° C. for 12 h to obtain high-purity nickel carbonate.
[0064] Comparative Example 1
[0065] A method for preparing nickel carbonate, which is different from Example 1 only in that ammonium oleate is not added.
[0066] Comparative Example 2
[0067] A method for preparing nickel carbonate, which is different from Example 1 only in that ammonium oleate is replaced by oleic acid.
[0068] In order to more clearly illustrate the content of the present invention, the purity and particle size of the nickel carbonate prepared in Examples 1-3 and Comparative Examples 1-2 of the present invention were tested, and the results are shown in Table 1:
[0069] Table 1 Detection results of nickel carbonate obtained by different methods
[0070] purity(%) Average particle size (μm) Example 1 99.5 3.4 Example 2 99.2 3.7 Example 3 99.6 3.3 Comparative Example 1 95.3 6.7 Comparative Example 2 96.8 5.1
[0071] From the test results in Table 1, it can be seen that the purity of the nickel carbonate prepared in Examples 1-3 of the present invention is higher than 99%, and can reach up to 99.6%, which is a high-purity standard; while the purity of Comparative Example 1-2 is slightly lower. In addition, the particle size of the nickel carbonate prepared in Examples 1-3 of the present invention is smaller than that of Comparative Example 1-2, indicating that the addition of ammonium oleate in the present invention also has an effect on the size of its particle size. The reason why the purity of Comparative Example 2 is lower and the particle size is slightly larger may be due to the poor dispersion effect of oleic acid in water.
[0072] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms should not be understood as necessarily being directed to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine different embodiments or examples described in this specification.
[0073] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A method for preparing high-purity nickel carbonate, characterized in that: The following steps are involved: Step 1, mixing a soluble nickel salt into deionized water, and stirring thoroughly until the nickel salt is uniformly dissolved to obtain a first mixed solution; Step 2, mixing ammonium bicarbonate, ammonium oleate and deionized water, and stirring them thoroughly to obtain a second mixed solution; Step 3, adding the second mixed liquid dropwise into the first mixed liquid to obtain a third mixed liquid; Step 4, pouring the third mixed liquid into a reactor, heating it, and after the reaction is completed, centrifuging and collecting the solid to obtain a crude product; Step 5, washing and drying the crude product in sequence to obtain high-purity nickel carbonate.
2. The method for preparing high-purity nickel carbonate according to claim 1, characterized in that: In step 1, the soluble nickel salt is a mixture of one or more of nickel sulfate, nickel nitrate and nickel chloride.
3. The method for preparing high-purity nickel carbonate according to claim 1, characterized in that: In step 1, the mass volume ratio of the soluble nickel salt to deionized water is (0.15-0.3) g:(20-40) mL.
4. The method for preparing high-purity nickel carbonate according to claim 1, characterized in that: In step 2, the mass volume ratio of ammonium bicarbonate, ammonium oleate and deionized water is (0.1-0.2) g: (0.5-1) g: (20-40) mL.
5. The method for preparing high-purity nickel carbonate according to claim 1, characterized in that: In step 3, the volume ratio of the first mixed liquid to the second mixed liquid is 1:1.1-1.
5.
6. The method for preparing high-purity nickel carbonate according to claim 1, characterized in that: In the step 3, after the dropwise addition is completed, stirring is continued for 10-20 minutes at a stirring speed of 100-200 r / min.
7. The method for preparing high-purity nickel carbonate according to claim 1, characterized in that: In step 4, the reaction temperature is 150-200° C. and the reaction time is 6-12 h.
8. The method for preparing high-purity nickel carbonate according to claim 1, characterized in that: In step 4, the centrifugal speed is 3000-5000 r / min.
9. The method for preparing high-purity nickel carbonate according to claim 1, characterized in that: In the step 5, washing is performed by washing three times with anhydrous ethanol and pure water in sequence, and drying is performed by vacuum drying at 40-60°C.
10. A high-purity nickel carbonate, characterized in that: The preparation method according to claim 1 is used for preparation.