A decorative film sheet for film outer decoration technology, a preparation method thereof, a corresponding thermal transfer ribbon and a preparation method thereof
Through thermal transfer technology and thermally cured resin carbon tape, the pattern is directly printed on the diaphragm, which solves the problem of high cost and low efficiency of decorative diaphragm in the outer mold decoration technology, and realizes efficient and personalized diaphragm production and simplifies The process flow and improve product performance.
Patent Information
- Application Number
- CN202211370519.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-03
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-11-03
AI Technical Summary
In the existing mold decoration technology, the import dependence of decorative diaphragms is high, expensive and limited production capacity. The traditional coating ink pattern is low and cannot meet personalized needs. The ultraviolet curing process is cumbersome and light pollution problems exist.
Decorative diaphragms are made using thermal transfer technology, and the three primary color ribbons are printed through a thermal transfer machine with three print heads. The pattern is printed directly on the diaphragm. Combined with the thermal curing resin carbon ribbon, the ultraviolet irradiation curing process is omitted, and the process is simplified. process.
It significantly improves the efficiency and personalization of the diaphragm, reduces production costs, simplifies the process flow, improves the scratch resistance and solvent resistance of the pattern, and reduces the risk of light pollution.
Smart Images

Figure CN115742617B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of film external decoration, and in particular relates to a decorative film sheet used for film external decoration technology, a preparation method thereof, a corresponding thermal transfer ribbon and a preparation method thereof. Background Art
[0002] The out-of-mold decoration technology is to wrap the decorated parts with 3D shapes with decorative films by heating and vacuum pressurization. The film coated with adhesive is tightly fitted to the surface of the processed parts. The pattern style on the film can achieve the appearance texture and effect of imitation wood grain, high gloss, imitation electroplating, imitation carbon fiber, imitation metal, etc. The out-of-mold decoration technology currently has no major problems in terms of equipment. The difficulty that has prevented the large-scale application of this process is mainly due to the high dependence on imports of decorative films, high prices, and limited production capacity. Its principle is as follows Figure 1 shown.
[0003] The existing decorative films used for off-mold decoration technology mostly use screen printing or color printing to apply ink patterns, and after the decorative film is coated on the substrate, the ink is mostly cross-linked by UV curing. This traditional method has two disadvantages. One is that different surface decorative patterns need to be individually engraved with screen rollers or plate making, resulting in low efficiency and failure to meet personalized needs. In addition, the subsequent UV curing process is not only cumbersome but also has problems such as light pollution. Summary of the invention
[0004] In order to solve the deficiencies of the prior art, the present invention provides a decorative film for film outer decoration technology, a preparation method thereof, a corresponding thermal transfer ribbon and a preparation method thereof. The technical solution provided by the present invention combines thermal transfer technology, which greatly improves the efficiency of film production and the degree of personalization of film patterns; the corresponding use of thermal curing resin ribbons saves the subsequent ultraviolet irradiation curing process, thereby simplifying the film outer decoration process. This new decorative film is expected to replace the currently imported decorative film, providing the possibility for large-scale application of this technology.
[0005] The technical solution provided by the present invention is as follows:
[0006] A decorative film sheet used in the film outer decoration technology comprises a release paper, an adhesive layer, a substrate and a base coating layer used for printing a thermal transfer pattern which are arranged in sequence.
[0007] Based on the above technical solution, a thermal transfer machine with at least three print heads is used to print three primary color ribbons. Through program control, any pattern can be printed on the base coating of the decorative film used for external film decoration technology provided by the present invention to form a complete decorative film that can be used for external film decoration.
[0008] Further, the thickness of the substrate is 5-30 μm, and the substrate can be one of polyacrylonitrile-butadiene-styrene (ABS) film, polyethylene terephthalate (PET) film, 1,4-polycyclohexylene dimethylene terephthalate film, polyethylene naphthalate (PEN) film, polyphenylene sulfide film, polystyrene (PS) film, polypropylene (PP) film, polyethylene (PE) film, polyvinyl chloride film, nylon film, polyimide film, etc., preferably with a thickness of 10-20 μm.
[0009] Furthermore, the thickness of the primer layer is 3-10 μm. The purpose of the primer layer is to connect the pattern layer and the substrate. A resin with excellent adhesion to the substrate and good printing capacity is selected. This type of resin can be exemplified by one or more combinations of acrylic resin, chlorinated polypropylene, polyurethane resin, epoxy resin, polyester resin, etc. The thickness is preferably 3-6 μm.
[0010] The preparation method of the primer layer is as follows: the above materials are dissolved in 2-butanone and toluene to prepare a primer liquid, and then the primer liquid is coated on the substrate by a 35-120-line ceramic anilox roller and a gravure coater, and then dried at 60-100°C.
[0011] Furthermore, the thickness of the bonding layer is 0.5-2 μm, preferably 0.5-1.0 μm. The bonding layer is composed of one or more polymer resins such as epoxy resin, ethylene-vinyl acetate copolymer, polyester resin, (meth) acrylic resin, polyolefin resin, polyurethane resin, vinyl chloride vinyl acetate, etc., and the bonding layer also contains 1-10 wt% of a silane coupling agent.
[0012] The bonding layer is prepared by dissolving the above materials with 2-butanone and toluene, and then preparing a bonding layer coating liquid, coating the bonding layer on the opposite side of the base coating with a 100-250-line ceramic anilox roller and a gravure coater, and drying at 60-100°C.
[0013] Furthermore, the thickness of the release paper is 20-50 um, and the release paper is attached to the adhesive layer during the coating process, which can prevent the front and back sides from sticking to each other after being rolled up and placed for a long time.
[0014] The present invention also provides a thermal transfer ribbon that can be used with the decorative film sheet used for the above-mentioned external film decoration technology, including a back coating layer, a substrate, a release layer and a pigment layer that can be thermally transferred to the base coating of the decorative film sheet used for the external film decoration technology.
[0015] Based on the above technical solution, a thermal transfer machine with at least three print heads and the above three primary color ribbons provided by the present invention are used, and any pattern can be printed onto the base coating of the above decorative film through program control, thereby preparing a complete decorative film that can be used for external decoration of the film.
[0016] Further, the thermal transfer ribbon substrate is selected from one of polyethylene terephthalate (PET) film, 1,4-polycyclohexylene dimethylene terephthalate film, polyethylene naphthalate (PEN) film, polyphenylene sulfide film, polystyrene (PS) film, polypropylene (PP) film, polyethylene (PE) film, polyvinyl chloride film, nylon film, polyimide film, etc., preferably with a thickness of 4-20um;
[0017] Furthermore, the release layer has a thickness of 0.05-0.5um, preferably 0.1-0.3um. The release layer can help the pigment layer transfer, improve the transfer ability, and prevent the pigment layer from sticking to the substrate when heated. At the same time, the thickness of the release layer and the choice of resin type can improve the scratch resistance and solvent resistance of the transferred pattern;
[0018] The main component of the release layer is one or more of polyester resin, acrylic resin (Tg>100°C), and EVA resin, and the balance is one or more of polyethylene glycol, carnauba wax, PE wax, and EVA wax, with a content of 5-10%.
[0019] The preparation method of the release layer is as follows: the above materials are dissolved in 2-butanone and toluene to prepare a back coating liquid, and then the back coating liquid is coated on the substrate by a 200-250 line ceramic anilox roller and a gravure coater, and then dried at 60-100°C.
[0020] Furthermore, the pigment layer has a thickness of 0.3-1.2 μm, preferably 0.5-1.0 μm. The pigment layer is composed of one or more polymer resins such as polyester resin, (meth) acrylic resin, polyurethane resin, fluorocarbon resin, ethylene-vinyl acetate copolymer, etc., with a content of 60-80%.
[0021] The pigment layer also contains inorganic pigments such as titanium white, cobalt blue, and carbon black, with a content of 5-10%;
[0022] The pigment layer also needs to add a cross-linking agent such as an isocyanate compound, with a content of 10-35%.
[0023] The pigment layer is prepared by dissolving the above materials with 2-butanone and toluene to prepare a back coating liquid, and then coating the back coating liquid on the substrate with a 200-250-line ceramic anilox roller and a gravure coater, and drying at 60-100°C.
[0024] Furthermore, the back coating layer has a thickness of 0.5-1.2 μm. The purpose of the back coating layer is to prevent the adverse effects such as stickiness or wrinkles caused by the temperature-sensitive heating head during thermal transfer. The wear-resistant thermal transfer coating comprises cellulose acetate propionate resin, polyurethane-modified silicone resin, acrylic acid-modified silicone resin, polyvinyl acetal resin, and polyvinyl butyral resin, with a content of 60-80%. The thickness is preferably 0.4-0.6 μm.
[0025] The back coating often needs to include inorganic particles such as talc, kaolin, calcium carbonate, aluminum hydroxide, silicon dioxide, graphite, boron nitride, etc., with a content of 5-10%.
[0026] The back coating layer often needs to contain one or more of a leveling agent, a dispersant and an antistatic agent, with a content of 1-5%.
[0027] The back coating often needs to add a cross-linking agent such as an isocyanate compound, with a content of 5-35%.
[0028] The preparation method of the back coating layer is as follows: the above materials are dissolved in 2-butanone and toluene to prepare a back coating liquid, and then the back coating liquid is coated on the substrate by a 200-250 line ceramic anilox roller and a gravure coater, and then dried at 60-100°C.
[0029] The present invention combines thermal transfer technology, and the resin-based carbon ribbon of the three primary colors is printed onto the decorative film through a thermal transfer machine with three print heads. This method can realize any pattern and any color combination, instead of adopting the traditional technical solution of separate plate making for a single pattern, which greatly improves the production efficiency and the degree of product personalization; in addition, the resin-based carbon ribbon disclosed in the present invention adopts a thermal curing method to replace the traditional ultraviolet curing technology, and a cross-linking reaction occurs during the heating of the print head and the subsequent heating of the decorative film and the bonding process of the substrate, thereby improving the scratch resistance and solvent resistance of the surface ink. In addition, the cross-linking reaction also helps to improve the adhesion between the ink and the film substrate so that it is not easy to fall off. The use of the thermal curing technology of the present invention to replace the traditional ultraviolet curing simplifies the production process and improves production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 It is a schematic structural diagram of the decorative film provided by the present invention with a pattern layer formed thereon.
[0031] Figure 2 It is a schematic diagram of the structure of the thermal transfer ribbon provided by the present invention.
[0032] Figure 3 The present invention is a schematic diagram of a preparation process of the decorative film provided by the present invention.
[0033] Figure 4The present invention is a schematic diagram of a preparation process of the thermal transfer ribbon provided by the present invention.
[0034] Figure 5 Schematic diagram of the membrane outer decoration technology in the prior art.
[0035] Attached Figure 1 , 2 The structures represented by the labels are listed below:
[0036] 1. Substrate; 2. Base coating; 3. Pattern layer; 4. Adhesive layer; 5. Release paper; 11. Substrate; 12. Release layer; 13. Pigment layer; 14. Back coating. DETAILED DESCRIPTION
[0037] The principles and features of the present invention are described below. The examples are only used to explain the present invention and are not used to limit the scope of the present invention. The materials used in the examples are all commercially available unless otherwise specified.
[0038] In a specific embodiment, Figure 1 As shown, the decorative film sheet for film outer decoration technology comprises a release paper 5, an adhesive layer 4, a substrate 1 and a base layer 2 for printing a thermal transfer pattern arranged in sequence. A thermal transfer machine with at least three print heads is used to print three primary color ribbons, and a pattern layer 3 is formed on the base layer of the decorative film sheet for film outer decoration technology to prepare a complete decorative film that can be used for film outer decoration.
[0039] In another specific embodiment, Figure 2 As shown, the thermal transfer ribbon comprises a back coating layer 14, a substrate 11, a release layer 12 and a pigment layer 13 which can be thermally transferred to the base coating layer of the decorative film sheet used for the film outer decoration technology. A thermal transfer machine with at least three print heads and the above three primary color ribbons are used to form a pattern layer on the base coating layer of the above decorative film, thereby preparing a complete decorative film that can be used for film outer decoration.
[0040] Example 1
[0041] Decorative films for external film decoration technology
[0042] Its material composition is:
[0043] The release paper material uses glassine release paper with a release force of 100g;
[0044] The bonding layer material is specifically 85 parts of epoxy resin, 10 parts of polyester resin, and 5 parts of silane coupling agent;
[0045] The base material is specifically polyacrylonitrile-butadiene-styrene (ABS) film;
[0046] The primer material specifically includes 90 parts of polyurethane resin and 10 parts of chlorinated polypropylene.
[0047] The preparation process is:
[0048] 1) Obtain a substrate material with a thickness of 25 um;
[0049] 2) 20 parts of the primer material were dissolved in 40 parts of 2-butanone and 40 parts of toluene to prepare a primer liquid, and then the primer liquid was coated on one side of the substrate material using a 40-line ceramic anilox roller and a gravure coater, and dried at 100° C. The specific thickness was 8 μm;
[0050] 3) 20 parts of the bonding layer material were dissolved in 40 parts of 2-butanone and 40 parts of toluene, and then prepared into a bonding layer coating liquid, and the bonding layer was coated on the other side of the base material by a 120-line ceramic anilox roller and a gravure coater, and dried at 100° C. The specific thickness was 2 μm;
[0051] 4) Lay the release paper on the adhesive layer to obtain a decorative film sheet for external film decoration technology.
[0052] Example 2
[0053] Decorative films for external film decoration technology
[0054] Its material composition is:
[0055] The release paper material uses glassine release paper with a release force of 100g;
[0056] The bonding layer material is specifically 85 parts of epoxy resin, 10 parts of ethylene-vinyl acetate copolymer, and 5 parts of silane coupling agent;
[0057] The base material is specifically polyacrylonitrile-butadiene-styrene (ABS) film;
[0058] The primer material specifically includes 90 parts of polyurethane resin and 10 parts of chlorinated polypropylene.
[0059] The preparation process is:
[0060] 1) Obtain a substrate material with a thickness of 25 um;
[0061] 2) 20 parts of the primer material were dissolved in 40 parts of 2-butanone and 40 parts of toluene to prepare a primer liquid, and then the primer liquid was coated on one side of the substrate material using a 40-line ceramic anilox roller and a gravure coater, and dried at 100° C. The specific thickness was 8 μm;
[0062] 3) 20 parts of the bonding layer material were dissolved in 40 parts of 2-butanone and 40 parts of toluene, and then prepared into a bonding layer coating liquid, and the bonding layer was coated on the other side of the base material by a 120-line ceramic anilox roller and a gravure coater, and dried at 100° C. The specific thickness was 2 μm;
[0063] 4) Lay the release paper on the adhesive layer to obtain a decorative film sheet for external film decoration technology.
[0064] Example 3
[0065] Decorative films for external film decoration technology
[0066] Its material composition is:
[0067] The release paper material uses glassine release paper with a release force of 100g;
[0068] The bonding layer material is specifically 85 parts of epoxy resin, 10 parts of polyester resin, and 5 parts of silane coupling agent;
[0069] The base material is specifically polyacrylonitrile-butadiene-styrene (ABS) film;
[0070] The primer material specifically includes 90 parts of polyurethane resin and 10 parts of vinyl chloride vinyl acetate resin.
[0071] The preparation process is:
[0072] 1) Obtain a substrate material with a thickness of 25 um;
[0073] 2) 20 parts of the primer material were dissolved in 40 parts of 2-butanone and 40 parts of toluene to prepare a primer liquid, and then the primer liquid was coated on one side of the substrate material using a 40-line ceramic anilox roller and a gravure coater, and dried at 100° C. The specific thickness was 8 μm;
[0074] 3) 20 parts of the bonding layer material were dissolved in 40 parts of 2-butanone and 40 parts of toluene, and then prepared into a bonding layer coating liquid, and the bonding layer was coated on the other side of the base material by a 120-line ceramic anilox roller and a gravure coater, and dried at 100° C. The specific thickness was 2 μm;
[0075] 4) Lay the release paper on the adhesive layer to obtain a decorative film sheet for external film decoration technology.
[0076] Example 4
[0077] Thermal transfer ribbon
[0078] Its material composition is:
[0079] The back coating material specifically includes 60% cellulose acetate propionate resin, 30% isocyanate curing agent, 5% talcum powder, 3% dispersant and 2% phosphate;
[0080] The substrate is specifically a polyethylene terephthalate (PET) film;
[0081] The release layer material specifically includes 80% polyester and 20% polyethylene glycol;
[0082] The pigment layer material specifically includes 60% polyester, 20% polyurethane, 15% blocked isocyanate, and 5% pigment;
[0083] The preparation process is:
[0084] 1) Obtaining a matrix material;
[0085] 2) A total of 10 parts of release layer material were dissolved in 45 parts of 2-butanone and 45 parts of toluene to prepare a back coating liquid, and then the back coating liquid was coated on one side of the substrate using a 250-line ceramic anilox roller and a gravure coater, and dried at 100° C. The specific thickness was 0.2 μm;
[0086] 3) A total of 20 parts of the pigment layer material were dissolved in 40 parts of 2-butanone and 40 parts of toluene to prepare a back coating liquid, and then the pigment layer liquid was coated on the release layer using a 230-line ceramic anilox roller and a gravure coater, and dried at 100°C to a thickness of 0.8um.
[0087] 4) A total of 20 parts of the back coating material were dissolved in 40 parts of 2-butanone and 40 parts of toluene to prepare a back coating liquid, and then a 250-line ceramic anilox roller and a gravure coater were used to coat the back coating liquid on the other side of the substrate, and dried at 100°C to a thickness of 0.4 um; a thermal transfer ribbon was obtained.
[0088] Example 5
[0089] Thermal transfer ribbon
[0090] Its material composition is:
[0091] The back coating material specifically includes 60% cellulose acetate propionate resin, 30% isocyanate curing agent, 5% talcum powder, 3% dispersant and 2% phosphate;
[0092] The substrate is specifically a polyethylene terephthalate (PET) film;
[0093] The release layer material specifically includes 80% polyester and 20% polyethylene glycol;
[0094] The pigment layer material specifically includes 60% polyester, 20% acrylic resin, 15% blocked isocyanate, and 5% pigment;
[0095] The preparation process is:
[0096] 1) Obtaining a matrix material;
[0097] 2) A total of 10 parts of release layer material were dissolved in 45 parts of 2-butanone and 45 parts of toluene to prepare a back coating liquid, and then the back coating liquid was coated on one side of the substrate using a 250-line ceramic anilox roller and a gravure coater, and dried at 100° C. The specific thickness was 0.2 μm;
[0098] 3) A total of 20 parts of the pigment layer material were dissolved in 40 parts of 2-butanone and 40 parts of toluene to prepare a back coating liquid, and then the pigment layer liquid was coated on the release layer using a 230-line ceramic anilox roller and a gravure coater, and dried at 100°C to a thickness of 0.8um.
[0099] 4) A total of 20 parts of the back coating material were dissolved in 40 parts of 2-butanone and 40 parts of toluene to prepare a back coating liquid, and then a 250-line ceramic anilox roller and a gravure coater were used to coat the back coating liquid on the other side of the substrate, and dried at 100°C to a thickness of 0.4 um; a thermal transfer ribbon was obtained.
[0100] Example 6
[0101] Thermal transfer ribbon
[0102] Its material composition is:
[0103] The back coating material specifically includes 60% cellulose acetate propionate resin, 30% isocyanate curing agent, 5% talcum powder, 3% dispersant and 2% phosphate;
[0104] The substrate is specifically a polyethylene terephthalate (PET) film;
[0105] The release layer material specifically includes 80% polyester and 20% polyethylene glycol;
[0106] The pigment layer material specifically includes 40% polyester, 40% polyurethane, 15% blocked isocyanate, and 5% pigment;
[0107] The preparation process is:
[0108] 1) Obtaining a matrix material;
[0109] 2) A total of 10 parts of release layer material were dissolved in 45 parts of 2-butanone and 45 parts of toluene to prepare a back coating liquid, and then the back coating liquid was coated on one side of the substrate using a 250-line ceramic anilox roller and a gravure coater, and dried at 100° C. The specific thickness was 0.2 μm;
[0110] 3) A total of 20 parts of the pigment layer material were dissolved in 40 parts of 2-butanone and 40 parts of toluene to prepare a back coating liquid, and then the pigment layer liquid was coated on the release layer using a 230-line ceramic anilox roller and a gravure coater, and dried at 100°C to a thickness of 0.8um.
[0111] 4) A total of 20 parts of the back coating material were dissolved in 40 parts of 2-butanone and 40 parts of toluene to prepare a back coating liquid, and then a 250-line ceramic anilox roller and a gravure coater were used to coat the back coating liquid on the other side of the substrate, and dried at 100°C to a thickness of 0.4 um; a thermal transfer ribbon was obtained.
[0112] Application Examples
[0113] The following combinations were printed using the self-developed soft label printer from Hunan Dingyiyuan Technology Development Co., Ltd. with a density of 100 and a speed of 20 cm / s:
[0114] The thermal transfer ribbon of Example 4 is used to print on the decorative film of Example 1 to obtain a decorative film material 1;
[0115] The thermal transfer ribbon of Example 4 is used to print on the decorative film of Example 2 to obtain a decorative film material 2;
[0116] The thermal transfer ribbon of Example 4 is used to print on the decorative film of Example 3 to obtain a decorative film material 3.
[0117] The thermal transfer ribbon of Example 5 is used to print on the decorative film of Example 3 to obtain a decorative film material 4;
[0118] The thermal transfer ribbon of Example 6 is used to print on the decorative film of Example 3 to obtain a decorative film material 5.
[0119] After the above decorative film materials are attached to the surface of the glass substrate using the outer film decoration technology, the adhesion, water boiling resistance, alcohol solvent resistance, and gasoline solvent resistance performance tests are carried out; the adhesion is based on "GB9286-1998 Scratching Test for Paint and Varnish Films", the water boiling resistance condition is 80℃ pure water bath for 30 minutes, and then the adhesion is tested according to the adhesion test standard, alcohol resistance is to soak the non-woven fabric with alcohol, apply a 1kg weight on the non-woven fabric and rub it back and forth on the pattern surface, and observe that the pattern has no discoloration or shedding after 50 back and forth times, which is qualified, and the gasoline solvent resistance test is the same as the alcohol solvent resistance test, that is, replace alcohol with gasoline; the results are shown in the following table:
[0120] Performance Testing Adhesion Resistant to boiling Alcohol solvent resistance Gasoline solvent resistant Decorative film materials1 Level 0 Level 1 qualified Failure Decorative film materials 2 Level 1 Level 2 qualified Failure Decorative film materials 3 Level 0 Level 1 qualified qualified Decorative film materials 4 Level 0 Level 1 Failure qualified Decorative film materials 5 Level 0 Level 1 qualified Failure
[0121] It can be seen from the above results that the decorative film material (or the pattern layer on the decorative film material) obtained by adopting the technical solution of the present invention can meet the adhesion standard requirements of "GB9286-1998 Scratching test for paint and varnish films", and has ideal solvent resistance and water boiling resistance.
[0122] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A decorative film for outer film decoration technology, characterized in that: It includes a release paper, an adhesive layer, a substrate and a primer layer for printing a thermal transfer pattern which are arranged in sequence; The bonding layer material is composed of 85 parts of epoxy resin, 10 parts of polyester resin and 5 parts of silane coupling agent; The matrix material is polyacrylonitrile-butadiene-styrene film; The base coating material is composed of 90 parts of polyurethane resin and 10 parts of vinyl chloride vinyl acetate resin; The thickness of the primer layer is 8 μm.
2. A method for preparing a decorative film sheet for external film decoration technology according to claim 1, characterized in that: The following steps are involved: 1) Obtaining the base material; 2) dissolving the primer material with 2-butanone and toluene to prepare a primer liquid, and then coating the primer liquid on one side of the substrate material using a 35-120-line ceramic anilox roller and a gravure coater, and drying at 60-100° C.; 3) The material of the bonding layer is dissolved in 2-butanone and toluene, and then prepared into a bonding layer coating liquid, and the bonding layer is coated on the other side of the base material by a ceramic anilox roller with 100-250 lines and a gravure coater, and then dried at 60-100°C; 4) Attach the release paper to the adhesive layer to obtain a decorative film sheet for external film decoration technology.