A new waterproof material suitable for deep and large vertical shafts and its preparation method and application
Through the foaming reaction of polyether polyol and polymethylene polyphenyl isocyanate, the problem of insufficient performance of concrete waterproof materials in the construction of deep and large shafts is solved, and a new type of highly efficient and corrosion-resistant waterproof material is provided, which is suitable for deep shaft construction. The construction of large shafts achieves excellent waterproofing effects and mechanical properties.
Patent Information
- Application Number
- CN202211482703.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-24
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-11-24
AI Technical Summary
In the construction of deep and large shafts, existing concrete waterproof materials cause water leakage due to structural defects, affecting the progress and safety of the project. Moreover, their mechanical properties and corrosion resistance are insufficient, making it difficult to meet special needs.
A new type of waterproof material is prepared using the foaming reaction of low molecular weight polyether polyol and polymethylene polyphenyl isocyanate, including component A and component B. It is synthesized through a one-step method and has excellent waterproofness, mechanical properties and Corrosion-resistant materials.
This new waterproof material has efficient waterproof performance, strong mechanical properties and corrosion resistance, is suitable for the construction of deep and large shafts, has a simple process and low cost, and is suitable for large-scale production and application.
Smart Images

Figure CN115746255B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of waterproof materials, and in particular relates to a new waterproof material suitable for deep and large vertical shafts, a preparation method and application thereof. Background Art
[0002] During the construction of deep and large vertical shafts, due to the large excavation depth, high soil pressure and high groundwater head, engineering accidents such as leakage often occur. Excessive water not only seriously affects the progress of the project, but also accelerates the deterioration of concrete and the corrosion of steel structures, affecting the service life and safety of the shaft.
[0003] In general shaft construction projects, the initial support of concrete also has a waterproofing function. However, due to the shortcomings of the concrete structure, such as large particles, low early strength, and long curing time, it is inevitable that cracks and fissures will occur. These cracks are exactly the seepage paths of groundwater, and some may even further develop into permeable pipes, endangering the safety of the shaft. Therefore, the existing use of concrete as a deep well waterproofing material can no longer meet the demand.
[0004] In summary, how to develop a new material with simple process, short curing time, high early strength, good mechanical properties, corrosion resistance and good waterproofness in view of the particularity of waterproof construction of deep and large vertical shafts is an urgent problem to be solved by technical personnel in this field. Summary of the invention
[0005] The purpose of the present invention is to provide a new waterproof material suitable for deep and large vertical shafts. The waterproof material with excellent performance can be obtained by using low molecular weight polyether polyol as the main raw material of component B and polymethylene polyphenyl isocyanate of component A to foam.
[0006] The raw materials used in the invention are low-cost, easy to purchase, and environmentally friendly. Through a one-step synthesis method, a waterproof material suitable for deep and large vertical shaft construction operations can be obtained, which has good waterproofness, short reaction time, excellent mechanical properties, strong corrosion resistance, and high foaming rate.
[0007] To achieve the above object, the present invention provides a new waterproof material suitable for deep and large vertical shafts.
[0008] Calculated by weight, it includes component A and component B, wherein:
[0009] Component A includes:
[0010] 100 parts of polymethylene polyphenyl isocyanate;
[0011] Component B includes:
[0012] 45-65 parts of polyether tetraol;
[0013] 35-55 parts of polyether triol;
[0014] 1.8-2.2 parts of catalyst;
[0015] 1.8 to 2.2 parts of chain extension crosslinking agent;
[0016] 3-4 parts of foam stabilizer;
[0017] Flame retardant 10 parts;
[0018] 0.6 to 1 part of foaming agent.
[0019] In a preferred embodiment, the weight ratio of component A to component B is 1:(0.65-0.75).
[0020] In a preferred embodiment, the molecular weight of the polyether tetraol in component B is 500, and the molecular weight of the polyether triol is 550.
[0021] In a preferred embodiment, the polyether tetraol in component B is polyether 4110G, and the polyether triol is polyether GP-305.
[0022] In a preferred embodiment, the catalyst includes one or two of dibutyltin dilaurate and 33% concentration of triethylenediamine;
[0023] The chain extending cross-linking agent includes one or two of 1,4-butanediol and triethanolamine;
[0024] The foam stabilizer is 201 methyl silicone oil;
[0025] The flame retardant is trichloropropyl phosphate;
[0026] The foaming agent is distilled water.
[0027] In a preferred embodiment, the catalyst is composed of dibutyltin dilaurate and 33% concentration of triethylenediamine in a mass ratio of 1: (0.4-0.55);
[0028] The chain extension cross-linking agent is composed of 1,4-butanediol and triethanolamine in a mass ratio of 1: (0.9-1.1).
[0029] Another object of the present invention is to provide a method for preparing a novel waterproof material suitable for deep and large vertical shafts, wherein the polyether polyol in component B is mixed and dried, and then stirred with other components at room temperature. The overall preparation method is simple and efficient, the mixing can be completed at room temperature, the equipment and energy consumption requirements are low, the preparation process is highly safe, and it is particularly suitable for large-scale industrial production.
[0030] To achieve the above object, the present invention provides a method for preparing a new waterproof material suitable for deep and large vertical shafts, which specifically comprises the following steps:
[0031] (1) Weighing the polyether tetraol and polyether triol in component B by weight, mixing at room temperature, and drying to obtain a mixed polyether polyol;
[0032] (2) Add a catalyst, a chain extender, a cross-linking agent, a foam stabilizer, a foaming agent and a flame retardant to the mixed polyether polyol, and stir evenly at room temperature to obtain component B.
[0033] In a preferred embodiment, in step (1), the drying treatment conditions are: drying at 40-60° C. for 12-24 hours.
[0034] Another object of the present invention is to provide an application method of a new waterproof material suitable for deep and large vertical shafts, which only requires pouring component A and component B into a foaming machine at the construction site to foam a mixed slurry, and then pouring the mixed slurry between the vertical shaft and the supporting structure to form a waterproof material. The application method is simple, has few requirements on environmental and equipment conditions, and is widely applicable to various deep well operation environments.
[0035] To achieve the above object, the present invention provides an application method of a new waterproof material suitable for deep and large vertical shafts, which specifically comprises the following steps:
[0036] At the construction site, component A and component B are respectively poured into a two-component foaming machine, and a mixed slurry is obtained through the foaming reaction. The mixed slurry is then injected into the space between the shaft and the supporting structure through the grouting holes to foam and generate waterproof materials specially designed for deep and large shafts.
[0037] In a preferred embodiment, the new waterproof material for deep and large vertical shafts is applicable to a well depth of up to 475m, a ground stress of up to 14.46MPa, and a foaming temperature of 30-80°C.
[0038] Compared with the prior art, the technical solution of the present invention has the following advantages:
[0039] The raw materials used in the present invention are all low-cost and easy to purchase; the preparation process adopts a one-step synthesis method, has a streamlined process, a stable process, low requirements on equipment and energy consumption, and is conducive to large-scale production and preparation.
[0040] The novel waterproof material provided by the present invention has the advantages of strong corrosion resistance, strong mechanical properties, good waterproofness, etc., has a simple application method, and is suitable for backfilling of deep and large vertical shaft walls to play the role of waterproofing and toughness support. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] These and / or other aspects and advantages of the present invention will become more clear and easier to understand from the following detailed description of the embodiments of the present invention in conjunction with the accompanying drawings, in which:
[0042] Figure 1This is the effect of component A and component B at different ratios on the yield strength of the material.
[0043] Figure 2 The main reactions involved in the synthesis of the deep and large vertical shaft waterproofing material of the present invention are (a) the reaction of isocyanate with polyol; and (b) the reaction of isocyanate with water.
[0044] Figure 3 Figure 3 shows the effect of catalyst on the material at different ratios, including (a), (b), and (c) micrographs and pore size distribution of waterproof materials when the mass ratio of dibutyltin dilaurate to A33 is 5:2; 2:1; and 5:3, respectively; (d), (e), and (f) are the corresponding particle size distribution diagrams; (g) the normal distribution diagram of the pore size of the three materials on the number of groups; (h) the effect of the amount of mixed catalyst on the solidification time when the mass ratio of dibutyltin dilaurate to A33 is 2:1. DETAILED DESCRIPTION
[0045] In order to enable those skilled in the art to better understand the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and specific implementation methods, but it should be understood that the protection scope of the present invention is not limited to the specific implementation methods.
[0046] The embodiment of the present invention solves the problems of poor waterproofing effect and low mechanical properties of materials in the prior art during construction of deep and large vertical shafts by providing a new waterproof material suitable for deep and large vertical shafts and a preparation method and application thereof.
[0047] The technical solution in the present invention is to solve the above problems, and the overall idea is as follows:
[0048] The present invention provides a novel waterproof material suitable for deep and large vertical shafts, which comprises component A and component B by weight, wherein:
[0049] Component A includes:
[0050] 100 parts of polymethylene polyphenyl isocyanate;
[0051] Component B includes:
[0052] 45-65 parts of polyether tetraol;
[0053] 35-55 parts of polyether triol;
[0054] 1.8-2.2 parts of catalyst;
[0055] 1.8 to 2.2 parts of chain extension crosslinking agent;
[0056] 3-4 parts of foam stabilizer;
[0057] Flame retardant 10 parts;
[0058] 0.6 to 1 part of foaming agent.
[0059] In a preferred embodiment, the weight ratio of component A to component B is 1:(0.65-0.75). Using the raw materials and dosage of component B in Example 2, while keeping other conditions unchanged, only the mass ratio of component A to component B is adjusted to test the difference in mechanical properties of the prepared waterproof material. The results are as follows: Figure 1 As shown. Figure 1 It can be seen that the yield strength of the material increases with the increase of density, but too high density will lead to large foam brittleness. Therefore, in order to take into account the mechanical properties and waterproof properties of the material, the mass of component A and component B is set to 1: (0.65-0.75).
[0060] In a preferred embodiment, the molecular weight of the polyether tetraol in component B is 500, and the molecular weight of the polyether triol is 550; preferably, the polyether tetraol in component B is polyether 4110G, and the polyether triol is polyether GP-305.
[0061] The two low molecular weight polyols selected in the present invention have similar structures and similar molecular weights, and the two have good mutual solubility. The polyether triol has lower viscosity and lower functionality, while the polyether tetraol has higher viscosity and higher functionality. The combination of the two takes into account both material properties while facilitating the control of reaction activity and being easy to operate.
[0062] In a preferred embodiment, the catalyst includes one or two of dibutyltin dilaurate and 33% concentration of triethylenediamine;
[0063] The chain extending cross-linking agent includes one or two of 1,4-butanediol and triethanolamine;
[0064] The foam stabilizer is 201 methyl silicone oil;
[0065] The flame retardant is trichloropropyl phosphate;
[0066] The foaming agent is distilled water.
[0067] In the present invention, the catalyst used is used to control the synthesis speed of the material. The catalyst includes one or more of dibutyltin dilaurate and 33% concentration of triethylenediamine. This is because the synthesis of the material mainly involves two chemical reactions: gel reaction and foaming reaction, such as Figure 2 As shown in the figure, only when the reaction process of the two reactions is in a good equilibrium state, the resulting material has good performance. Experiments have shown that tin-based catalysts have a significant effect on promoting the gel reaction of the material, while amine catalysts have a significant catalytic effect on the foaming reaction. The reasonable combination of the two can not only control the material synthesis speed, but also optimize the pore morphology and improve the mechanical properties of the foam.
[0068] Preferably, the catalyst is composed of dibutyltin dilaurate and 33% triethylenediamine in a mass ratio of 1: (0.4-0.55). Using the raw materials and dosages in Example 2, only the ratio of dibutyltin dilaurate and A33 in the catalyst is changed to verify the effect of the catalyst on the material. The results are as follows: Figure 3 As shown in the figure, it can be seen that the material slices obtained within this ratio range all show the characteristics of good pore uniformity and high roundness. Therefore, it can be determined that the above catalyst ratio can make the gel reaction and foaming reaction during the synthesis of the waterproof material reach the best balance state.
[0069] In the present invention, the chain extension cross-linking agent used includes one or two of 1,4-butanediol and triethanolamine. These two materials are small molecular materials with binary and ternary structures respectively, and the hydroxyl groups contained therein can react with the isocyanate in the polyisocyanate, so as to promote the cross-linking of the long-chain carbamate groups formed by the reaction of the isocyanate and the polyol to form a spatial grid structure, thereby making the material have higher strength and better mechanical properties.
[0070] Preferably, the chain extender crosslinker is composed of 1,4-butanediol and triethanolamine in a mass ratio of 1: (0.9-1.1). It has been verified through compression tests that, under the premise that other conditions remain unchanged, the chain extender crosslinker component and dosage are within the above range, the compressive strength of the foam is the highest, which indirectly reflects that the mesh structure of the synthetic space of the waterproof material is optimal.
[0071] In the present invention, the foam stabilizer used is 201 methyl silicone oil, which can effectively reduce the surface tension in the reaction system, thereby reducing the energy required for free gas dispersion. On the other hand, it can also increase the early viscosity of the foam mixture, thereby improving the early stability of the foam and improving the cell quality.
[0072] When the foam temperature rises, it is easy to ignite, especially in a deep well environment, which is very likely to cause danger. Therefore, the flame retardant used in the present invention is trichloropropyl phosphate, which can utilize the phosphorus-containing segment degradation to produce water-absorbing polyphosphoric acid during the temperature rise reaction, dehydrate the foam and carbonize it, and then generate a dense phosphorus-containing carbon layer to block the transfer of internal and external heat and the propagation of oxygen, and at the same time, it will also produce non-combustible gases such as CO2, reduce the concentration of combustible gases, and then achieve a good flame retardant effect, improve the reaction safety, and be more conducive to deep and large vertical shaft environment operations.
[0073] In the present invention, the foaming agent used is distilled water; the principle is that the hydroxyl group in the water reacts with the isocyanate group in the polyisocyanate to generate carbon dioxide gas, thereby generating bubbles in the liquid material, causing the material volume to expand and achieve the foaming effect. Moreover, compared with the commonly used low-boiling point physical foaming agent, distilled water as a foaming agent has zero pollution to the environment, low cost, and is safer in the foaming reaction in the deep well environment.
[0074] Another object of the present invention is to provide a method for preparing a new waterproof material suitable for deep and large vertical shafts, which specifically comprises the following steps:
[0075] (1) Weighing the polyether tetraol and polyether triol in component B by weight, mixing at room temperature, and drying to obtain a mixed polyether polyol;
[0076] (2) Add a catalyst, a chain extender, a cross-linking agent, a foam stabilizer, a foaming agent and a flame retardant to the mixed polyether polyol, and stir evenly at room temperature to obtain component B.
[0077] In the present invention, component A is only polymethylene polyphenyl isocyanate, which can be directly purchased from outside, and the preparation steps are omitted. In component B, since there is moisture in the polyether polyol used in industry, and water is used as a foaming agent in the present invention, in order to accurately control the amount of raw materials and ensure the product effect, it is necessary to first mix the low molecular weight polyol, dry it to remove moisture, and then mix it with other raw materials to prepare component B. The prepared component B has good stability, is easy to store and transport, and can be sold separately as a commercial product.
[0078] In a preferred embodiment, in step (1), the drying treatment conditions are: drying at 40-60° C. for 12-24 hours, and more preferably, the drying device is a vacuum dryer. After drying under such conditions, the properties of the polyether polyol are not affected, and the internal moisture can be fully removed to avoid affecting the reaction effect when blending with other raw materials.
[0079] Another object of the present invention is to provide an application method of a new waterproof material suitable for deep and large vertical shafts, which specifically comprises the following steps:
[0080] At the construction site, component A and component B are respectively poured into a two-component foaming machine, and a mixed slurry is obtained through the foaming reaction. The mixed slurry is then injected into the space between the shaft and the supporting structure through the grouting holes to foam and generate waterproof materials specially designed for deep and large shafts.
[0081] In a preferred embodiment, the new waterproof material for deep and large vertical shafts is applicable to a well depth of up to 475 m, a ground stress of up to 14.46 MPa, and a foaming temperature of 30-90°C.
[0082] In a preferred embodiment, the foaming flow rate is 20 to 24 L / min.
[0083] The technical solution of the present application is described in detail below through specific embodiments:
[0084] Unless otherwise specified, the technical means used in the present invention are conventional means well known to those skilled in the art, and the various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0085] In the present invention, the polymethylene polyphenyl isocyanate used, the product name is PAPI, purchased from Yantai Wanhua Polyurethane Co., Ltd.; the polyether triol used is polyether GP-305, purchased from Shandong Dongda Bluestar Co., Ltd.; the polyether tetraol used is polyether 4110G, 33% concentration of triethylene diamine product name is A33, 1,4-butanediol, triethanolamine, dibutyltin dilaurate are all purchased from Xuzhou Yihuiyang New Materials Co., Ltd.
[0086] In the present invention, parts by weight may be μg, mg, g, kg, or other weight units known in the art, or multiples thereof, such as 1 / 10, 1 / 100, 10 times, 100 times, etc. In the present invention, the normal temperature is 25±5°C.
[0087] Example 1
[0088] S1, 65g of polyether tetraol and 35g of polyether triol were mixed at room temperature, and placed in a dryer at 60°C for drying and dehydration for 24 hours to obtain a mixed polyether polyol;
[0089] S2, adding 1.26g of dibutyltin dilaurate and 0.54g of A33 solution to form 1.8g of catalyst, 0.94g of 1,4-butanediol and 0.86g of triethanolamine to form 1.8g of chain extender crosslinker, 3.0g of foam stabilizer, 0.6g of foaming agent, 10g of flame retardant to the dried mixed polyether polyol, stirring at room temperature to obtain component B;
[0090] S3. Mix component A (polymethylene polyphenyl isocyanate) and component B at a mass ratio of 1:0.65 at 30°C, stir with a stirrer at a rate of 200 r / min for 30 seconds, and then pour into a mold to obtain a waterproof material suitable for deep well operations.
[0091] Example 2
[0092] S1, 50g of polyether tetraol and 50g of polyether triol were mixed at room temperature, and placed in a dryer at 60°C for drying and dehydration for 24 hours to obtain a mixed polyether polyol;
[0093] S2, adding 1.2g of dibutyltin dilaurate and 0.6g of A33 solution to the dried mixed polyether polyol to form 1.8g of catalyst, 0.9g of 1,4-butanediol and 0.9g of triethanolamine to form 1.8g of chain extender crosslinker, 3.0g of foam stabilizer, 0.6g of foaming agent, and 10g of flame retardant, and stirring evenly at room temperature to obtain component B;
[0094] S3. Mix component A (polymethylene polyphenyl isocyanate) and component B at a mass ratio of 1:0.7 at 30°C, stir with a stirrer at a rate of 200 r / min for 30 seconds, and then pour into a mold to obtain a waterproof material suitable for deep well operations.
[0095] Example 3
[0096] S1, 45g of polyether tetraol and 55g of polyether triol were mixed at room temperature, and placed in a dryer at 60°C for drying and dehydration for 24 hours to obtain a mixed polyether polyol;
[0097] S2, adding 1.16g of dibutyltin dilaurate and 0.64g of A33 solution to form 1.8g of catalyst, 0.86g of 1,4-butanediol and 0.94g of triethanolamine to form 1.8g of chain extender crosslinker, 3.0g of foam stabilizer, 0.6g of foaming agent, 10g of flame retardant to the dried mixed polyether polyol, stirring evenly at room temperature to obtain component B;
[0098] S3. Mix component A (polymethylene polyphenyl isocyanate) and component B at a mass ratio of 1:0.75 at 30°C, stir with a stirrer at a rate of 200 r / min for 30 seconds, and then pour into a mold to obtain a waterproof material suitable for deep well operations.
[0099] Example 4
[0100] S1, 50g of polyether tetraol and 50g of polyether triol were mixed at room temperature, and placed in a dryer at 60°C for 24 hours to obtain a mixed polyether polyol;
[0101] S2, adding 1.46g of dibutyltin dilaurate and 0.74g of A33 solution to the dried mixed polyether polyol, 2.2g of catalyst, 1.1g of 1,4-butanediol and 1.1g of triethanolamine, 2.2g of chain extender crosslinker, 4.0g of foam stabilizer, and 0.8g of foaming agent, and stirring evenly at room temperature to obtain component B;
[0102] S3. Mix component A (polymethylene polyphenyl isocyanate) and component B in a mass ratio of 1:0.75 at 30°C, stir with a stirrer at a rate of 200 r / min for 30 seconds, and then pour into a mold to obtain a waterproof material suitable for deep well operations.
[0103] Example 5
[0104] In Example 2, the mixing temperature of step S3, component A (polymethylene polyphenyl isocyanate) and component B was adjusted to 60° C., and the rest was completely consistent with Example 2.
[0105] Effect example
[0106] The technical effects of the waterproof materials obtained in test examples 1, 2, 3 and 4 are as follows:
[0107] Measure the density of materials according to GB / T 6343-2009;
[0108] Measure the setting time of materials according to JC / T 2041-2010;
[0109] Measure the tensile strength of materials according to GB / T9641-1998;
[0110] Measure the 10% compressive strength of the material according to GB / T8813-2020;
[0111] Determine the material permeability coefficient based on the field test of the borehole water pressure test in the Engineering Geology Handbook;
[0112] The acid and alkali resistance of the material is tested according to the specification GB / T1763.
[0113] The specific test results are shown in Table 1:
[0114] Table 1
[0115]
[0116] It can be seen from Table 1 that under normal temperature of 30°C and conventional operating temperature of 60°C, the new waterproof material provided by the present invention has good waterproof performance, fast reaction time, excellent mechanical properties, strong corrosion resistance, high foaming rate and other characteristics. The raw materials used are easy to purchase and low cost, and the preparation process is simple, with low requirements for equipment and energy consumption, and has the advantages of reducing costs and increasing efficiency. It is very suitable for waterproofing projects of deep and large vertical shafts. Compared with the higher foaming temperature in the prior art, the material prepared by the present invention can have a good foaming effect at room temperature.
[0117] Comparative Example 1
[0118] S1. Place 100 g of polyether tetraol in a dryer at 60° C. and dry for 24 hours;
[0119] S2, adding 1.2g of dibutyltin dilaurate and 0.6g of A33 solution to the dried polyether tetraol to form 1.8g of catalyst, 0.9g of 1,4-butanediol and 0.9g of triethanolamine to form 1.8g of chain extender crosslinker, 3.0g of foam stabilizer, 0.6g of foaming agent, and 10g of flame retardant, and stirring evenly at room temperature to obtain component B;
[0120] S3. Mix component A (polymethylene polyphenyl isocyanate) and component B at a mass ratio of 1:0.7 at 30°C, stir with a stirrer at a rate of 200 r / min for 30 seconds, and then pour into a mold to obtain a waterproof material suitable for deep well operations.
[0121] Under the experimental conditions, no polyether triol was added, only polyether tetraol was added, and the prepared waterproof material was brittle and had a density of 0.33 kg / m 3 , much higher than that in the example, the tensile strength is 0.52 MPa, and powdering damage occurs during the compression test, and the flexibility is much lower than that in the example. This is because the functionality of the polyether tetraol is too large, and the reaction rate of isocyanate and polyether tetraol is too fast, which hinders the generation of bubbles in the material, resulting in fewer and uneven foam pores, which in turn leads to a larger material density and poor flexibility.
[0122] Comparative Example 2
[0123] S1. Mix 50g of polyether tetraol and 50g of polyether triol at room temperature, and place in a dryer at 60°C for 24 hours for drying and dehydration;
[0124] S2, adding 0.6g of dibutyltin dilaurate and 1.2g of A33 solution to the dried polyether tetraol to form 1.8g of catalyst, 0.9g of 1,4-butanediol and 0.9g of triethanolamine to form 1.8g of chain extender crosslinker, 3.0g of foam stabilizer, 0.6g of foaming agent, and 10g of flame retardant, and stirring evenly at room temperature to obtain component B;
[0125] S3. Mix component A (polymethylene polyphenyl isocyanate) and component B at a mass ratio of 1:0.7 at 30°C, stir with a stirrer at a rate of 200 r / min for 30 seconds, and then pour into a mold to obtain a waterproof material suitable for deep well operations.
[0126] Under the experimental conditions, the ratio of dibutyltin dilaurate and A33 is seriously unbalanced, the resulting waterproof material has coarse pores, and it is impossible to make tensile specimens. When subjected to force, it is powdered and damaged. This is because the amount of A33 used is large and the amount of dibutyltin dilaurate used is small, resulting in the gel reaction speed being slower than the foaming reaction, that is, the formed gel cannot carry bubbles, resulting in a large number of bubbles escaping or gathering, which in turn increases the material density, coarse pores, and is prone to powder damage.
[0127] Comparative Example 3
[0128] S1. Mix 50g of polyether tetraol and 50g of polyether triol at room temperature, and place in a dryer at 60°C for 24 hours for drying and dehydration;
[0129] S2, adding 2.4g of dibutyltin dilaurate and 1.2g of A33 solution to the dried polyether tetraol to form 3.6g of catalyst, 0.9g of 1,4-butanediol and 0.9g of triethanolamine to form 1.8g of chain extender crosslinker, 3.0g of foam stabilizer, 0.6g of foaming agent, and 10g of flame retardant, and stirring evenly at room temperature to obtain component B;
[0130] S3. Mix component A (polymethylene polyphenyl isocyanate) and component B at a mass ratio of 1:0.7 at 30°C, stir with a stirrer at a rate of 200 r / min for 30 seconds, and then pour into a mold to obtain a waterproof material suitable for deep well operations.
[0131] Under the experimental conditions, the amount of catalyst used seriously exceeded the standard. After the A and B components were mixed, they reacted violently, generating a large amount of heat instantly. The resulting waterproof material was easily crushed under stress and had poor mechanical properties. In addition, there were risks such as clogging of the grouting pipe during actual construction. This was because the increase in catalyst content and the increase in reaction speed caused the chemical energy that should have been generated within a few minutes to be released within a few seconds, resulting in heat accumulation and temperature surges, resulting in the lack of flexibility of the formed waterproof material, and in severe cases even fire.
[0132] Comparative Example 4
[0133] S1. Mix 50g of polyether tetraol and 50g of polyether triol at room temperature, and place in a dryer at 60°C for 24 hours for drying and dehydration;
[0134] S2, adding 1.2g of dibutyltin dilaurate and 0.6g of A33 solution to the dried polyether tetraol to form 1.8g of catalyst, 0.9g of 1,4-butanediol and 0.9g of triethanolamine to form 1.8g of chain extender crosslinker, without using foam stabilizer, 0.6g of foaming agent, and 10g of flame retardant, stirring evenly at room temperature to obtain component B;
[0135] S3. Mix component A (polymethylene polyphenyl isocyanate) and component B at a mass ratio of 1:0.7 at 30°C, stir with a stirrer at a rate of 200 r / min for 30 seconds, and then pour into a mold to obtain a waterproof material suitable for deep well operations.
[0136] Under this set of experimental conditions, no foam stabilizer was used. As a result, components A and B could not expand after being mixed. This is because the foam stabilizer can reduce the surface tension in the reaction system, thereby reducing the energy required for the dispersion of free gases and increasing the early viscosity of the foam mixture. The lack of foam stabilizer will cause the gas to escape and the material will be unable to expand.
[0137] Comparative Example 5
[0138] S1. Mix 50g of polyether tetraol and 50g of polyether triol at room temperature, and place in a dryer at 60°C for 24 hours for drying and dehydration;
[0139] S2. Add 1.2g of dibutyltin dilaurate and 0.6g of A33 solution to the dried polyether tetraol to form 1.8g of catalyst, 0.9g of 1,4-butanediol and 0.9g of triethanolamine to form 1.8g of chain extender crosslinker, 3% of foam stabilizer, 1.8g of foaming agent, and 10g of flame retardant, and stir evenly at room temperature to obtain component B;
[0140] S3. Mix component A (polymethylene polyphenyl isocyanate) and component B in a mass ratio of 1:0.7 at 30°C, use a stirrer to stir at a rate of 200 r / min for 30 seconds, and then pour into a mold to obtain a waterproof material suitable for deep well operations.
[0141] Under this set of experimental conditions, the amount of foaming agent used seriously exceeded the standard, and the density of the waterproof material produced was 0.0821Kg / m 3 , the yield strength is 1.21MPa, the tensile strength is 1.97MPa, which is much lower than that of the embodiment; and its permeability coefficient is 4.3110 -5 cm / s, which is much higher than that in the example. This is because the amount of foaming agent used increases, the amount of carbon dioxide generated increases, the bubbles aggregate and cause the cells to become coarse, the expansion rate of the foam increases, the density decreases, the mechanical properties decrease, and the permeability coefficient increases.
[0142] The foregoing description of specific exemplary embodiments of the present invention is for the purpose of illustration and demonstration. These descriptions are not intended to limit the present invention to the precise form disclosed, and it is clear that many changes and variations can be made based on the above teachings. The purpose of selecting and describing the exemplary embodiments is to explain the specific principles of the present invention and its practical application, so that those skilled in the art can realize and utilize various different exemplary embodiments of the present invention and various different selections and changes. The scope of the present invention is intended to be limited by the claims and their equivalents.
Claims
1. A waterproof material suitable for deep and large vertical shafts, characterized in that: Calculated by weight, it includes component A and component B, wherein: Component A includes: 100 parts of polymethylene polyphenyl isocyanate; Component B includes: 45-65 parts of polyether tetraol; 35-55 parts of polyether triol; 1.8-2.2 parts of catalyst; 1.8-2.2 parts of chain extension crosslinking agent; 3~4 parts of foam stabilizer; Flame retardant 10 parts; 0.6~1 part of foaming agent; The catalyst is composed of dibutyltin dilaurate and 33% triethylenediamine in a mass ratio of 1: (0.4-0.55); The foaming agent is distilled water.
2. The waterproof material suitable for deep and large vertical shafts as claimed in claim 1, characterized in that: The weight ratio of component A to component B is 1:(0.65-0.75).
3. The waterproof material suitable for deep and large vertical shafts as claimed in claim 1, characterized in that: The molecular weight of the polyether tetraol in component B is 500, and the molecular weight of the polyether triol is 550.
4. The waterproof material suitable for deep and large vertical shafts as claimed in claim 3, characterized in that: The polyether tetraol in component B is polyether 4110G, and the polyether triol is polyether GP-305.
5. The waterproof material suitable for deep and large vertical shafts according to claim 1, characterized in that: The chain extending cross-linking agent includes one or two of 1,4-butanediol and triethanolamine; The foam stabilizer is 201 methyl silicone oil; The flame retardant is trichloropropyl phosphate.
6. The waterproof material suitable for deep and large vertical shafts as claimed in claim 5, characterized in that: The chain extension cross-linking agent is composed of 1,4-butanediol and triethanolamine in a mass ratio of 1: (0.9-1.1).
7. The method for preparing a waterproof material suitable for a deep and large vertical shaft according to any one of claims 1 to 6, characterized in that: The following steps are involved: (1) Weighing the polyether tetraol and polyether triol in component B according to weight, mixing at room temperature, and drying to obtain a mixed polyether polyol; (2) Add a catalyst, a chain extender, a cross-linking agent, a foam stabilizer, a foaming agent and a flame retardant to the mixed polyether polyol and stir evenly at room temperature to obtain component B.
8. The method for preparing waterproof material suitable for deep and large vertical shafts according to claim 7, characterized in that: In step (1), the drying treatment conditions are: drying at 40-60° C. for 12-24 hours.
9. The method for applying the waterproof material suitable for deep and large vertical shafts as claimed in any one of claims 1 to 6 or the waterproof material prepared by the method of any one of claims 7 to 8, characterized in that: The following steps are involved: At the construction site, component A and component B are respectively poured into a two-component foaming machine, and a mixed slurry is obtained through the foaming reaction. The mixed slurry is then injected into the space between the shaft and the supporting structure through the grouting holes to foam and generate waterproof material specially designed for deep and large shafts.
10. The application method according to claim 9, characterized in that: The waterproof material for the deep and large vertical shaft is applicable to a well depth of up to 475m, a ground stress of up to 14.46MPa, and a foaming temperature of 30-80°C.
Citation Information
Patent Citations
Halogen-free flame-retardant rigid polyurethane foamed plastic and preparation method for same
CN103694438A
All-water-foamed and high-strength polyurethane grouting uplift material with high construction environment adaptability and low grout viscosity and preparation method of polyurethane grouting uplift material
CN106432685A