A method for delaying the degradation rate of magnesium alloys
By forming a gallium-magnesium alloy layer on the surface of magnesium alloy, the problems of fast degradation rate and uneven degradation products of magnesium alloy are solved, the corrosion resistance and wear resistance of magnesium alloy are improved, the degradation rate is delayed, and it is suitable for bone heal.
Patent Information
- Application Number
- CN202211485139.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-24
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-11-24
AI Technical Summary
Magnesium alloys degrade rapidly in bone implants and the degradation products are uneven, leading to an increase in the pH value of the local environment in the body.
By forming a gallium-magnesium alloy layer with high microhardness, good wear resistance and corrosion resistance on the surface of the magnesium alloy, using methyl silicone oil or glycerol as the melting medium, and mechanically stirring the gallium oxide and magnesium alloy to form a pre-oxidized Gallium coating, and controlling the thickness of the alloying layer by adjusting the alloying time to delay the degradation rate of the magnesium alloy.
It effectively reduces the corrosion current density and voltage of magnesium alloy, improves its corrosion resistance and wear resistance, and delays the degradation rate of magnesium alloy, making it suitable for the growth and healing of different bones.
Smart Images

Figure HDA0003961871610000011 
Figure HDA0003961871610000012 
Figure HDA0003961871610000021
Abstract
Description
Technical Field
[0001] The invention relates to a method for delaying the degradation rate of a magnesium alloy, and belongs to the technical field of magnesium alloy surface treatment. Background Art
[0002] Magnesium alloys are used as temporary load-bearing orthopedic implants in bone implantology. As the healing process progresses, they gradually dissolve in the human body. In addition, magnesium alloys have good biocompatibility and are lightweight, making them potential candidates for the development of biodegradable implant materials. However, in actual medical applications, magnesium alloys have problems such as fast degradation rate and uneven degradation products. At the same time, the large amount of gas generated will cause the pH value of the local environment in the body to increase.
[0003] To address these problems, the surface of magnesium alloys needs to be modified. Commonly used magnesium alloy surface modification technologies include alloying, chemical conversion, vapor deposition, anodizing, electroplating, laser surface treatment and ion implantation. Among them, alloying is currently the main measure to improve the degradation behavior of magnesium alloys. For example, although magnesium-neodymium alloys have good mechanical properties, they still have the problem of fast degradation rate. Summary of the invention
[0004] Aiming at the problem that the existing magnesium alloy has poor surface corrosion resistance and fast degradation rate, the present invention proposes a method for delaying the degradation rate of the magnesium alloy. The present invention adopts methyl silicone oil or glycerin as a smelting medium, alloys the pre-oxidized gallium obtained by stirring gallium oxide with the magnesium alloy, and forms an alloying layer with high microhardness, good wear resistance and corrosion resistance, and good bonding force on the surface of the magnesium alloy. By adjusting the alloying time, alloying layers of different thicknesses are obtained, thereby controlling the degradation rate of the magnesium alloy and making it suitable for the growth and healing of different bones.
[0005] A method for slowing down the degradation rate of magnesium alloy, the specific steps are as follows:
[0006] (1) grinding, polishing, cleaning and drying the surface of the magnesium alloy in sequence to obtain a pretreated magnesium alloy;
[0007] (2) heating the liquid metal gallium to 30-40° C. and mechanically stirring the pre-oxidation reaction to obtain pre-oxidized gallium;
[0008] (3) coating the pre-oxidized gallium on the surface of the pre-treated magnesium alloy to obtain a pre-oxidized gallium coating;
[0009] (4) The magnesium alloy coated with the pre-oxidized gallium coating is added to a smelting medium, wherein the smelting medium covers the magnesium alloy, and the temperature is uniformly raised to a preset temperature and kept at this temperature for smelting, and the smelting medium on the surface is cleaned, and the surface is ground, polished, cleaned and dried to obtain a surface-treated magnesium alloy.
[0010] The magnesium alloy in step (1) is a magnesium-aluminum-zinc magnesium alloy, a magnesium-zinc magnesium alloy or a rare earth magnesium alloy.
[0011] Preferably, the magnesium-aluminum-zinc magnesium alloy is AZ31 magnesium alloy or AZ91 magnesium alloy, the magnesium-zinc magnesium alloy is Mg-Zn magnesium alloy or ZK60 magnesium alloy, and the rare earth magnesium alloy is Mg-4.5Nd-0.5Zn-1Zr magnesium alloy.
[0012] The mechanical stirring rate of step (2) is 1200-1500 r / min, the oxidation reaction time is 10-15 hours, and the viscosity of the pre-oxidized gallium is 150-200 mPa.s.
[0013] The thickness of the gallium pre-oxidized coating in step (3) is 10 to 50 μm.
[0014] The smelting medium in step (4) is methyl silicone oil, high temperature chain oil, high temperature heat transfer oil, polyester oil (POE), polyalphaolefin (PAO) or polyphenyl-biphenyl ether, and the depth of the smelting medium submerging the magnesium alloy is 2 to 5 cm.
[0015] The preset temperature in step (4) is not higher than the boiling point of the smelting medium.
[0016] The preset temperature is 200-230° C., and the heat preservation melting time is 4-24 hours.
[0017] The principle of slowing down the degradation rate of magnesium alloy: the higher the corrosion potential, the smaller the corrosion tendency, and the lower the corrosion current density, the slower the material corrodes. The internal reason for the corrosion of magnesium alloy is the low electrochemical potential of metallic magnesium (-2.37V), while the electrochemical potential of gallium is (-0.55V), which is much higher than the electrochemical potential of magnesium. Therefore, the corrosion resistance of the surface is improved by alloying gallium with magnesium; secondly, compared with magnesium alloy, the number of highly active magnesium sites exposed on the surface of the gallium-magnesium alloy layer is significantly reduced, thereby alleviating the corrosion of the magnesium alloy. Therefore, the prepared gallium-magnesium alloy layer can protect the underlying magnesium alloy substrate from corrosion.
[0018] The beneficial effects of the present invention are:
[0019] (1) The present invention uses pre-oxidized gallium after mechanical stirring, and the viscosity is 150-300 mPa.s, which enhances the adhesion between the liquid metal gallium and the magnesium alloy substrate, is easy to coat, and makes the process simpler;
[0020] (2) The present invention uses methyl silicone oil, glycerin and other smelting media to avoid oxidation during the alloying process, and the prepared gallium-magnesium alloy layer has the characteristics of good corrosion resistance and wear resistance;
[0021] (3) The present invention uses liquid metal gallium to form a surface alloy. Gallium is easy to alloy with metals and is non-toxic. The generated intermetallic compounds can effectively solve the problem of fast degradation rate of magnesium alloys.
[0022] (4) The gallium-magnesium alloy layer of the present invention has good bonding strength with the magnesium alloy substrate, can effectively improve the surface strength of the magnesium alloy, and can also improve the surface wear resistance and corrosion resistance of the magnesium alloy. By adjusting the alloying time, alloying layers of different thicknesses can be obtained, thereby controlling the degradation rate of the magnesium alloy, making it suitable for the growth and healing of different bones. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The SEM and EDS images of the magnesium alloy for medical use and gallium alloyed for 12 hours in Example 1;
[0024] Figure 2 This is the XRD diagram of the magnesium alloy for medical use and gallium alloyed for 12 hours in Example 1;
[0025] Figure 3 The Tafel curve of the original sample of the magnesium alloy for medical use in Example 1 and the test after alloying with gallium for 12 hours;
[0026] Figure 4 The SEM and EDS images of the AZ31 magnesium alloy alloyed with gallium for 12 hours in Example 2;
[0027] Figure 5 is the XRD pattern of AZ31 magnesium alloy alloyed with gallium for 12h in Example 2;
[0028] Figure 6 The Tafel plot of the original AZ31 magnesium alloy and the gallium alloyed AZ31 magnesium alloy in Example 2 for 12 hours;
[0029] Figure 7 The SEM and EDS images of ZK60 magnesium alloy alloyed with gallium for 24 hours in Example 3;
[0030] Figure 8 is the XRD pattern of ZK60 magnesium alloy alloyed with gallium for 24 hours in Example 3;
[0031] Fig. 9 This is the Tafel plot of the ZK60 magnesium alloy in Example 3, which was the original sample and alloyed with gallium for 12 hours. DETAILED DESCRIPTION
[0032] The present invention is further described in detail below in conjunction with specific implementation modes, but the protection scope of the present invention is not limited to the described contents.
[0033] Embodiment 1: A method for slowing down the degradation rate of magnesium alloy, the specific steps are as follows:
[0034] (1) The surface of the magnesium alloy is polished with 400 mesh, 800 mesh, 1200 mesh and 2000 mesh metallographic sandpaper in sequence to remove surface pollutants; polished to a mirror surface, cleaned with ethanol, and dried to obtain a pretreated magnesium alloy; wherein the composition of the magnesium alloy is Nd 4.5%, Zn 0.5%, Zr 1%, and the rest is Mg in terms of mass percentage;
[0035] (2) heating the liquid metal gallium to 30° C. and performing a mechanical stirring pre-oxidation reaction at a speed of 1300 r / min for 12 h to obtain pre-oxidized gallium; the viscosity of the pre-oxidized gallium is 220 mPa.s;
[0036] (3) coating the pre-oxidized gallium on the surface of the pre-treated magnesium alloy to obtain a pre-oxidized gallium coating; the thickness of the pre-oxidized gallium coating is 30 μm;
[0037] (4) The magnesium alloy coated with the pre-oxidized gallium coating is added into a smelting medium (methyl silicone oil), wherein the smelting medium submerges the magnesium alloy to a depth of 4 cm, and the temperature is uniformly raised to a preset temperature of 220° C. and maintained at this temperature for 12 hours to alloy the alloy;
[0038] (5) After the smelting medium (methyl silicone oil) is cooled, the alloy is taken out, and the smelting medium (methyl silicone oil) on the surface is cleaned with an ethanol sodium hydroxide solution with a concentration of 1 mol / L, and the alloy is polished with 2000-mesh sandpaper to a mirror surface, and then cleaned with ethanol and dried to obtain a surface-treated magnesium alloy;
[0039] SEM and EDS images of medical magnesium alloy alloyed with gallium for 12 hours are shown in Figure 1 ,from Figure 1 It can be seen that for the sample alloyed with methyl silicone oil as the melting medium for 12 hours, the alloy layer is approximately in the range of 140 to 190 μm. The distribution of gallium and magnesium elements can be observed in the line scanning diagram; the XRD diagram of the medical magnesium alloy alloyed with gallium for 12 hours is shown in Figure 2 ,from Figure 2 It can be seen that gallium and magnesium alloying form intermetallic compounds; the Tafel curves of the original medical magnesium alloy and the gallium alloying test for 12 hours are shown in Figure 3 ,from Figure 3 It can be seen that the corrosion resistance test of the sample in SBF shows that the corrosion current density is increased from the original 0.589mA / cm 2 Reduced to 0.182mA / cm 2 The corrosion voltage increased from -1.31V to -1.15V, indicating that the degradation rate of the magnesium alloy decreased.
[0040] Embodiment 2: A method for slowing down the degradation rate of magnesium alloy, the specific steps are as follows:
[0041] (1) The surface of the magnesium alloy (AZ31 magnesium alloy) is polished with 400 mesh, 800 mesh, 1200 mesh and 2000 mesh metallographic sandpaper to remove surface pollutants; polished to a mirror surface, cleaned with ethanol, and dried to obtain a pretreated magnesium alloy; wherein the composition of the magnesium alloy (AZ31 magnesium alloy) is Al3.0%, Zn0.8%, and the rest is Mg in terms of mass percentage;
[0042] (2) heating the liquid metal gallium to 35° C. and performing a mechanical stirring pre-oxidation reaction at a speed of 1400 r / min for 15 h to obtain pre-oxidized gallium; the viscosity of the pre-oxidized gallium is 280 mPa.s;
[0043] (3) coating the pre-oxidized gallium on the surface of the pre-treated magnesium alloy to obtain a pre-oxidized gallium coating; the thickness of the pre-oxidized gallium coating is 50 μm;
[0044] (4) The magnesium alloy coated with the pre-oxidized gallium coating is added into a smelting medium (polyester oil POE), wherein the smelting medium submerges the magnesium alloy to a depth of 3 cm, and the temperature is uniformly raised to a preset temperature of 210° C. and maintained for 12 hours to alloy the alloy;
[0045] (5) After the smelting medium (polyester oil POE) is cooled, the alloy is taken out, and the smelting medium (polyester oil POE) on the surface is cleaned with an ethanol sodium hydroxide solution with a concentration of 1 mol / L, and the alloy is polished with 2000-mesh sandpaper to a mirror surface, and then cleaned with ethanol and dried to obtain a surface-treated magnesium alloy;
[0046] SEM and EDS images of AZ31 magnesium alloy alloyed with gallium for 12h are shown in Figure 4 ,from Figure 4 It can be seen that the alloy layer of the sample alloyed with polyester oil POE as the smelting medium for 12 hours is approximately in the range of 250 to 300 μm. The distribution of gallium and magnesium elements can be observed in the line scanning diagram; the XRD diagram of AZ31 magnesium alloy alloyed with gallium for 12 hours is shown in Figure 5 ,from Figure 5 It can be seen that gallium and magnesium alloying form intermetallic compounds; the Tafel curve of AZ31 magnesium alloy original sample and gallium alloying 12h test is shown in Figure 6 ,from Figure 6 It can be seen that the corrosion resistance test of the sample in SBF shows that the corrosion current density is increased from the original 0.724mA / cm 2 Reduced to 0.178mA / cm 2 , the corrosion voltage increased from -1.52V to -0.42V, indicating that the degradation rate of the magnesium alloy was reduced and the corrosion resistance was improved.
[0047] Embodiment 3: A method for slowing down the degradation rate of magnesium alloy, the specific steps are as follows:
[0048] (1) The surface of the magnesium alloy (ZK60 magnesium alloy) is polished with 400 mesh, 800 mesh, 1200 mesh and 2000 mesh metallographic sandpaper to remove surface pollutants; polished to a mirror surface, cleaned with ethanol, and dried to obtain a pretreated magnesium alloy; wherein the composition of the magnesium alloy (ZK60 magnesium alloy) is 5.32% Zn, 0.1% Zr, and the rest is Mg in terms of mass percentage;
[0049] (2) heating the liquid metal gallium to 40° C. and performing a mechanical stirring pre-oxidation reaction at a speed of 1500 r / min for 10 h to obtain pre-oxidized gallium; the viscosity of the pre-oxidized gallium is 160 mPa.s;
[0050] (3) coating the pre-oxidized gallium on the surface of the pre-treated magnesium alloy to obtain a pre-oxidized gallium coating; the thickness of the pre-oxidized gallium coating is 40 μm;
[0051] (4) The magnesium alloy coated with the pre-oxidized gallium coating is added into a smelting medium (poly-alpha-olefin PAO), wherein the smelting medium submerges the magnesium alloy to a depth of 5 cm, and the temperature is uniformly raised to a preset temperature of 230° C. and maintained for 12 hours to alloy the alloy;
[0052] (5) After the smelting medium (PAO) is cooled, the alloy is taken out, and the smelting medium (PAO) on the surface is cleaned with an ethanol sodium hydroxide solution with a concentration of 1 mol / L, and the alloy is polished with 2000-mesh sandpaper to a mirror surface, and then cleaned with ethanol and dried to obtain a surface-treated magnesium alloy;
[0053] SEM and EDS images of ZK60 magnesium alloy alloyed with gallium for 12h are shown in Figure 7 ,from Figure 7 It can be seen that the alloy layer of the sample alloyed with poly-alpha-olefin PAO as the melting medium for 12 hours is approximately in the range of 400-500 μm. The distribution of gallium and magnesium elements can be observed in the line scanning diagram; the XRD diagram of ZK60 magnesium alloy alloyed with gallium for 12 hours is shown in Figure 8 ,from Figure 8 It can be seen that gallium and magnesium alloying form intermetallic compounds; the Tafel curve of ZK60 magnesium alloy original sample and gallium alloying 12h test is shown in Fig. 9 ,from Fig. 9 It can be seen that the corrosion resistance test of the sample in SBF shows that the corrosion current density is increased from the original 0.076mA / cm 2 Reduced to 0.040mA / cm 2 The corrosion voltage increased from -1.49V to -0.28V, indicating that the degradation rate of the magnesium alloy was reduced and the corrosion resistance was improved.
[0054] The specific implementation modes of the present invention are described in detail above, but the present invention is not limited to the above implementation modes, and various changes can be made within the knowledge scope of ordinary technicians in this field without departing from the purpose of the present invention.
Claims
1. A method for slowing down the degradation rate of magnesium alloy, characterized in that: The specific steps are as follows: (1) grinding, polishing, cleaning and drying the surface of the magnesium alloy in sequence to obtain a pretreated magnesium alloy; (2) heating the liquid metal gallium to 30-40° C. and mechanically stirring the pre-oxidation reaction to obtain pre-oxidized gallium; the mechanical stirring rate is 1200-1500 r / min, the oxidation reaction time is 10-15 h, and the viscosity of the pre-oxidized gallium is 150-300 mPa.s; (3) coating the pre-oxidized gallium on the pre-treated magnesium alloy surface to obtain a pre-oxidized gallium coating; (4) The magnesium alloy coated with the pre-oxidized gallium coating is added to a smelting medium, wherein the smelting medium submerges the magnesium alloy, and the temperature is uniformly raised to a preset temperature and maintained for smelting, and the smelting medium on the surface is cleaned, and the surface is ground, polished, cleaned and dried to obtain a surface-treated magnesium alloy; the preset temperature is not higher than the boiling point of the smelting medium.
2. The method for slowing down the degradation rate of magnesium alloy according to claim 1, characterized in that: The magnesium alloy in step (1) is a magnesium-aluminum-zinc magnesium alloy, a magnesium-zinc magnesium alloy or a rare earth magnesium alloy.
3. The method for slowing down the degradation rate of magnesium alloy according to claim 2, characterized in that: The magnesium-aluminum-zinc magnesium alloy is AZ31 magnesium alloy or AZ91 magnesium alloy, the magnesium-zinc magnesium alloy is Mg-Zn magnesium alloy or ZK60 magnesium alloy, and the rare earth magnesium alloy is Mg-4.5Nd-0.5Zn-1Zr magnesium alloy.
4. The method for slowing down the degradation rate of magnesium alloy according to claim 1, characterized in that: The thickness of the gallium pre-oxidized coating in step (3) is 10 to 50 μm.
5. The method for slowing down the degradation rate of magnesium alloy according to claim 1, characterized in that: The smelting medium in step (4) is methyl silicone oil, high temperature chain oil, high temperature heat transfer oil, polyester oil, polyalphaolefin or polyphenyl-biphenyl ether, and the depth of the smelting medium covering the magnesium alloy is 2 to 5 cm.