Stretchable electronic materials with electromechanical dual heterogeneous structures and their preparation and application
By constructing a mechanical-electrical double heterostructure on a polymer-based fiber membrane, the problem of insufficient linearity and stability of electrical signals in a wide strain range of existing resistive stretchable strain sensors is solved, and a wide strain range is achieved. Linear resistive-mechanical strain response suitable for a variety of flexible electronic applications.
Patent Information
- Application Number
- CN202211257008.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-14
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-10-14
AI Technical Summary
Existing resistive stretchable strain sensors have insufficient electrical signal linearity and stability within a wide strain range, making it difficult to meet the needs of large-strain applications in the medical and health fields. Moreover, the preparation method lacks large-scale processing capabilities and controllable material structure.
A polymer-based fiber membrane is used to deposit conductive materials by spinning method. The thermodynamic partial compatibility and modulus difference of polymer 1 and polymer 2 are used, combined with the different interactions of conductive materials, to construct a mechanical-electrical double heterostructure. Achieve heterogeneous characterization of conductive properties and modulus, resulting in linear resistive-mechanical strain response over a wide strain range.
It broadens the linear resistance-strain response range within the strain range, improves sensitivity and interface stability, and achieves high linearity and strong stability of the flexible stretchable strain sensor, which is suitable for a variety of flexible electronic applications.
Smart Images

Figure CN115748246B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of polymer functional composite materials, and specifically relates to a flexible stretchable strain sensing material with mechanical-electrical dual heterostructure (mechanical-electrical dual heterostructure) characteristics and a preparation method thereof. The obtained strain sensing material has the characteristics of linear response of resistance with strain and adjustable strain sensitivity within a wide strain range.
[0002] Background technology introduction
[0003] The combination of the rapidly developing flexible electronic technology and smart medical care, remote real-time health management and artificial intelligence technology has led to an increasing demand for stretchable and wearable flexible sensing materials and devices in the consumer market. Among them, resistive strain sensors have good application prospects in application scenarios such as smart health, telemedicine, human-computer interaction and intelligent robots due to their advantages such as simple processing methods, strong material selectivity, and flexible and adjustable device performance. For the above-mentioned applications, it is crucial to be able to use resistive strain sensors to directly and simply monitor the strain of an object and accurately report the results, which requires the above-mentioned strain sensors to have linear resistance-strain response characteristics. Compared with traditional strain sensors, although resistive stretchable strain sensors based on polymer composites have a wide range of stretchable strains and good skin-fitting properties, their resistance often shows nonlinear response characteristics with strain, which is not convenient for signal acquisition and correction in actual applications. Therefore, it is very important to develop flexible stretchable strain sensors that have good conformality and fit with the service object, and whose resistance responds linearly with strain, to promote the integrated development of flexible electronic technology, the Internet of Things and artificial intelligence technology.
[0004] There are two main types of linear response strain sensors currently on the market, namely piezoelectric sensors and metal foil strain gauges. Although they both have the characteristic of linear response of electrical signals to strain, their strain monitoring range is very narrow (<10%), which makes it difficult to meet the large strain (~50%) application requirements in the medical and health field. In addition, the former has high preparation costs and poor skin fit, which seriously limits its practical application. The latter has a very limited strain range and extremely low sensitivity (strain sensitivity coefficient is about 1 to 2), so they are currently very limited in many flexible electronic applications. Although resistive polymer composite-based strain sensing materials have the characteristics of simple structure and scalable processing, the advantages of flexible design of shape as needed, and the characteristics of easy adjustment of strain range and sensitivity, their electrical signal linearity and stability are often very insufficient.
[0005] At present, most of the research work attempts to idealize the surface microstructure of the base material or use different resistors to alternately assemble to form a high-low resistance combined conductive network to synchronize the electrical signal response with the strain. However, the strain sensing materials prepared by the above methods can only achieve high electrical signal linearity within a very small strain range, and the preparation methods of such electronic materials have almost no large-scale processing capabilities, and the structural controllability of the materials at the microscopic scale is poor. Therefore, the stability and repeatability of its resistance-strain signal response are poor, and it is still a long way from practical application; this is one of the major technical challenges faced by the field of resistive stretchable strain sensors. Summary of the invention
[0006] In view of the shortcomings and limitations of the prior art, the present invention provides a micro / nanostructured flexible stretchable electronic fiber film material with dual heterogeneous properties of modulus and conductivity and a preparation method thereof. The prepared flexible stretchable electronic material has excellent inorganic-organic interface stability and good and stable linear resistance-mechanical strain response characteristics within a wide strain range; therefore, it can be used to prepare flexible stretchable strain sensors with good conformality and fit to the service object and linear resistance response to strain.
[0007] The technical solution of the present invention:
[0008] The first technical problem to be solved by the present invention is to provide a flexible and stretchable electronic material, wherein the flexible and stretchable electronic material is a conductive material deposited on the surface of a polymer-based fiber film;
[0009] The polymer-based fiber membrane is prepared by a spinning method in which the first solution is a core layer solution and the second solution is a sheath layer solution, wherein the first solution is a solution containing polymer 1, and the second solution is a solution containing polymer 1 and polymer 2, and the mass ratio of polymer 1 to polymer 2 in the second solution is 9:1 to 5:5;
[0010] Among them, the polymer 1 and polymer 2 are partially compatible in thermodynamics, the interactions between the polymer 1 and polymer 2 and the conductive material are different, the Young's modulus of polymer 2 is greater than that of polymer 1; and the polymer 1 is a thermoplastic elastomer, and the polymer 2 is a thermoplastic plastic.
[0011] Preferably, the mass ratio of polymer 1 to polymer 2 in the second solution is 8:2 to 5:5.
[0012] Furthermore, the different interactions between polymer 1 and polymer 2 and the conductive material refer to: different physical interactions between polymer 1 and polymer 2 and the conductive filler (specifically, interactions such as conjugated π electron-ion, π-π conjugation or van der Waals forces) or different chemical interactions; due to the different interactions between the two polymers and the conductive material (such as a large number of conjugated π bonds in the molecular structure of polymer 1 and isolated π bonds in the molecular structure of polymer 2), there is an obvious difference in surface concentration of the distribution of the conductive material in the two polymer microphases, which leads to a large difference in the conductivity of the conductive material in the two polymers (the conductivity difference is more than 10 times), so that the resulting stretched electronic material has heterogeneous conductive properties.
[0013] Furthermore, in the flexible stretchable electronic material, the ratio of the electrical conductivity of the polymer 1 microphase after the conductive material is deposited on the surface to the electrical conductivity of the polymer 2 after the conductive material is deposited on the surface is ≥10.
[0014] Furthermore, the polymer 1 is selected from: thermoplastic polystyrene-butadiene-styrene block copolymer (SBS), styrene-ethylene-butadiene-styrene block copolymer (SEBS) or styrene-isoprene-styrene triblock copolymer (SIS).
[0015] Furthermore, the polymer 2 is selected from: polystyrene (PS), plastics containing styrene or polypropylene (PP).
[0016] Furthermore, the styrene-containing plastic is at least one of acrylonitrile-butadiene-styrene copolymer (ABS) or styrene-acrylonitrile copolymer (SAN).
[0017] Preferably, the polymer 1 and polymer 2 are selected from the following combinations: SBS-PP, SBS-ABS, SBS-SAN, SIS-PS or SIS-SAN.
[0018] More preferably, the polymer 1 is a thermoplastic polystyrene-butadiene copolymer, and the polymer 2 is polystyrene.
[0019] Furthermore, the Young's moduli of polymer 1 and polymer 2 satisfy that the ratio of the Young's modulus of polymer 2 to the Young's modulus of polymer 1 is not less than 100.
[0020] Furthermore, the conductive material is metal nanoparticles or nanowires, one-dimensional or two-dimensional carbon-based conductive materials, or conductive polymers.
[0021] Furthermore, the metal in the metal nanoparticles or nanowires is silver, gold or copper.
[0022] Furthermore, the spinning method is a coaxial near-field electrostatic direct writing method, an electrostatic spinning method or a wet spinning method.
[0023] Furthermore, the solvent in the first solution and the second solution is selected from: a mixed solvent of toluene and ethylene dichloride, toluene or ethylene dichloride; preferably toluene.
[0024] Furthermore, the mass concentration of the first solution is 15-25%.
[0025] Furthermore, the mass concentration of the second solution is 10-25%.
[0026] The second technical problem to be solved by the present invention is to provide a method for preparing the above-mentioned flexible and stretchable electronic fiber membrane material, wherein the preparation method is: using existing methods (such as magnetron sputtering, spraying or in-situ reduction deposition) to deposit the conductive material on the surface of the polymer-based fiber membrane.
[0027] The third technical problem to be solved by the present invention is to point out the use of the above-mentioned flexible stretchable electronic fiber film material in the preparation of flexible stretchable strain sensing materials or strain sensors. The prepared flexible stretchable strain sensor has a linear response of resistance with strain and has good conformity and fit with the service object.
[0028] The fourth technical problem to be solved by the present invention is to provide a method for preparing a polymer-based membrane material, the preparation method being: preparing the material by spinning using a first solution as a core layer solution and a second solution as a sheath layer solution; the first solution is a solution containing only polymer 1, the second solution is a solution containing polymer 1 and polymer 2, and the mass ratio of polymer 1 to polymer 2 in the second solution is 9:1 to 4:6; wherein the polymer 1 and polymer 2 are partially compatible in thermodynamics, and the Young's modulus of polymer 2 is greater than that of polymer 1; and the polymer 1 is a thermoplastic elastomer, and the polymer 2 is a thermoplastic plastic.
[0029] Preferably, the mass ratio of polymer 1 to polymer 2 in the second solution is 8:2 to 5:5.
[0030] Furthermore, the Young's modulus of polymer 1 and polymer 2 satisfy: the ratio of the Young's modulus of polymer 2 to the Young's modulus of polymer 1 is not less than 100; in the present invention, the Young's modulus of the material is obtained by a tensile mechanics test at room temperature, with a loading rate of 50 mm / min, and the test reference is GB / T 1040.1.
[0031] Furthermore, the polymer 1 is selected from: thermoplastic polystyrene-butadiene-styrene block copolymer (SBS), styrene-ethylene-butadiene-styrene block copolymer (SEBS) or styrene-isoprene-styrene triblock copolymer (SIS).
[0032] Furthermore, the polymer 2 is selected from: polystyrene (PS), plastics containing styrene or polypropylene (PP).
[0033] Furthermore, the styrene-containing plastic is at least one of acrylonitrile-butadiene-styrene copolymer (ABS) or styrene-acrylonitrile copolymer (SAN).
[0034] Preferably, the polymer 1 and polymer 2 are selected from the following combinations: SBS-PP, SBS-ABS, SBS-SAN, SIS-PS or SIS-SAN.
[0035] More preferably, the polymer 1 is a thermoplastic polystyrene-butadiene copolymer, and the polymer 2 is polystyrene.
[0036] Furthermore, the microstructural feature of the polymer-based fiber membrane is that polymer 2 is distributed in the polymer 1 matrix as a dispersed phase.
[0037] Furthermore, there is a good interface between the dispersed phase polymer 2 and the matrix phase polymer 1: for example, the interfacial tensions are similar or the viscosity ratio is close to 1.
[0038] Furthermore, the spinning method is a coaxial near-field electrostatic direct writing method, an electrostatic spinning method or a wet spinning method.
[0039] Preferably, the spinning method is a coaxial near-field electrostatic direct writing method. During the coaxial near-field electrostatic direct writing process: the core-sheath layer spinning solution advancing speed: 1-10 mL / h (preferably 2-3 mL / h; voltage: 3-10 kV (preferably 4-6 kV); near-field electrostatic direct writing distance: 1-2 mm; time is determined according to the width and thickness of the film.
[0040] Furthermore, the solvent in the first solution and the second solution is selected from: a mixed solvent of toluene and ethylene dichloride (in any proportion), toluene or ethylene dichloride; preferably toluene.
[0041] Furthermore, in order to facilitate electrostatic direct writing and ensure that the prepared composite material forms the desired island-like dispersed morphology and has good mechanical properties, the mass concentration of the first solution is 15-25% (preferably 20%), and it can be used only after stirring at room temperature for 8 hours until the polymer is completely dissolved.
[0042] Furthermore, in order to ensure the smooth electrostatic direct writing process and the good fusion between the sheath solution and the core solution, the mass concentration of the second solution is 10-25% (preferably 20%), and it can be used only after stirring at room temperature for 8 hours until the polymer is completely dissolved.
[0043] The fifth technical problem to be solved by the present invention is to provide a polymer-based fiber membrane, which is prepared by the above method.
[0044] The sixth technical problem to be solved by the present invention is to point out the use of the above-mentioned polymer-based film in the preparation of flexible and stretchable electronic materials.
[0045] Beneficial effects of the present invention:
[0046] The elastomeric electronic fiber membrane material with mechanical-electrical dual heterogeneous structural characteristics prepared by the present invention has the following advantages:
[0047] 1) The present invention selects specific polymers 1 and 2: the two have a difference in modulus, are partially compatible in thermodynamics, and have different interactions with conductive fillers, resulting in significant differences in the distribution concentration of conductive fillers in the two polymers (the conductivity differs by more than 10 times), so the resulting stretched electronic material not only has a modulus heterogeneity, but also has a conductive property heterogeneity, that is, it has a double heterogeneous property structure. Since the functional electronic fiber membrane has a conductive property heterogeneity, the change in the conductive path caused by the growth of microcracks can keep pace with the change in strain; otherwise, the microcrack extension caused by the local stress concentration generated by the modulus heterogeneous microstructure is not enough to produce a linear resistance-strain response feature in a wide strain range; that is, the obtained stretched electronic material has a wide strain range (can exceed 50%, up to 80%), compared with the flexible stretchable electronic fiber membrane material provided by the prior art (the strain range of the provided stretched electronic material with a modulus heterogeneous structure is up to 25%), the linear resistance-strain response range is widened by 55%. The obtained flexible stretchable electronic material has excellent interface stability, good, stable and controllable linear resistance-mechanical strain response characteristics, and excellent and stable sensitivity within a wide strain loading range.
[0048] 2) The method for constructing the modulus difference and electrical difference type heterostructure of the electronic fiber membrane material of the present invention is simple and efficient, which has great advantages for constructing micro / nanoscale heterostructures on the surface of micro / nano fibers and is expected to be extended to more material structure design fields.
[0049] 3) The polymer-based fiber membrane obtained by the present invention is embedded with a large amount of micron-sized plastic (polystyrene) spherical dispersed phase, and the diameter of the dispersed phase varies with the mass fraction of polymer 1 and polymer 2, and can be regulated according to the interfacial tension interaction between the two, and the interface with polymer 1 is complete and stable.
[0050] 4) The resistance-mechanical strain performance of the electronic fiber obtained by the present invention presents a stable linear characteristic; and the size and density distribution of the dispersed phase on the fiber membrane surface can be adjusted by changing the mass ratio of the two polymers in the sheath mixed solution, thereby achieving performance regulation. BRIEF DESCRIPTION OF THE DRAWINGS
[0051] Figure 1 a and Figure 1 b is an electron microscope image of the surface structure of the fiber membrane obtained in Example 1 with a mass ratio of SBS to PS of 9:1 (i.e., fiber membrane SP91).
[0052] Figure 2 a and Figure 2 b is an electron microscope image of the surface structure of the fiber membrane with a mass ratio of SBS to PS of 8:2 (SP82) obtained in Example 2.
[0053] Figure 3 a is an electron microscope image of the surface structure of the fiber membrane with a mass ratio of SBS to PS of 7:3 (SP73) obtained in Example 3, Figure 3 b is Figure 3 A partial enlarged view of a.
[0054] Figure 4 a is an electron microscope image of the surface structure of the fiber membrane with a mass ratio of SBS to PS of 6:4 (SP64) obtained in Example 4, Figure 4 b is Figure 4 A partial enlarged view of a.
[0055] Figure 5 This is an electron microscope image of the surface structure of the fiber membrane with a mass ratio of SBS to PS of 5:5 (SP55) obtained in Example 5.
[0056] Figure 6 This is an electron microscope image of the surface structure of the SBS fiber membrane obtained in Comparative Example 1.
[0057] Figure 7 This is an electron microscope image of the surface structure of the fiber membrane obtained in Comparative Example 2 with a mass ratio of SBS to PS of 4:6 (SP46).
[0058] Figure 8 Electron microscope images of the distribution state of silver nanoparticles in SBS and PS phases in Example 4 at different magnifications.
[0059] Fig. 9 is the modulus of SBS and PS used in the examples ( Fig. 9 a) and loaded silver nanoparticles ( Fig. 9 b) Electrical conductivity results afterwards.
[0060] Fig.10 This is a graph showing the average particle size distribution of the dispersed phase polymer 2 in the matrix phase polymer 1 in Example 1, Example 2, Example 3, Example 4, and Example 5.
[0061] Fig.11This is a result diagram of the continuous sensitivity change trend of the flexible stretchable electronic materials obtained in Example 1, Example 2, Example 3, Example 4, Example 5, Comparative Example 1 and Comparative Example 2.
[0062] Fig.12 This is a graph showing the strain range test results of the flexible stretchable electronic fiber membrane material obtained in Example 2 of Chinese patent CN202111257899.1. DETAILED DESCRIPTION
[0063] Based on the idea of designing and modifying the interface between polymer flexible substrate materials and active conductive materials, the present invention derives a special structural design strategy that can plan the local mechanical and conductive properties of the substrate and conductive materials. This strategy, which has both mechanical and electrical heterogeneous structural characteristics, is expected to achieve the regulation of the mechanical and electrical response characteristics of stretchable strain sensing materials, synchronize the change in resistance with the development of strain, and achieve high linearity and strong stability of the sensor's electrical signal.
[0064] Based on the above design ideas, the present invention provides a flexible and stretchable electronic fiber membrane material, wherein the flexible and stretchable electronic fiber membrane material is a conductive material deposited on the surface of a polymer-based fiber membrane; the polymer-based fiber membrane is prepared by using polymer 1 and polymer 2 according to a certain method: first, the polymer 1 and polymer 2 selected by the present invention need to meet the following conditions: 1) There is a thermodynamically partial compatibility characteristic, and (micro) phase separation can occur; and the thermodynamic compatibility can effectively characterize the interface interaction, otherwise the mechanical properties of the material are very poor, it is difficult to ensure good stretchability, and it is also impossible to block the rapid expansion of microcracks, and it is difficult to achieve the goal of adjusting linearity and sensitivity; 2) The interactions between the two selected polymers and the selected conductive fillers are significantly different, resulting in obvious concentration differences in the distribution of the conductive material in the two polymer microphases (thus achieving the heterogeneous characteristics of conductive performance); 3) Polymer 1 and polymer 2 have different Young's moduli (achieving modulus heterogeneity). At the same time, the solution prepared by blending polymer 1 and polymer 2 according to a specific ratio (the mass ratio of polymer 1 to polymer 2 must be varied between 9:1 and 5:5) is used as a sheath solution (such as a mixed solution of SBS and PS can ensure good interface interaction between SBS and PS and obtain a double heterogeneous microstructure after being covered with a conductive filler), and the solution of polymer 1 is used as a core solution; ensuring surface microphase separation determines that the sheath is a two-phase system, and the core is pure SBS. In order to ensure the stretchability of the fiber (to ensure mechanical elasticity), if there is only a two-phase sheath with a phase-separated structure, the stretchability and recoverability of the fiber are poor. It can be seen that the present invention adopts a novel composite material processing method, and finally obtains a flexible stretchable electronic material with a mechanical and electrical double heterogeneous structure, realizes the regulation of the mechanical and electrical response characteristics of the stretchable strain sensing material, keeps the change of resistance synchronized with the development of strain, and realizes the high linearity and strong stability of the sensor electrical signal.
[0065] Thermodynamic compatibility in the present invention refers to the ability of the components of the blend to accommodate each other and form a macroscopically uniform material. For polymers, some polymers may have excellent compatibility, while other polymer pairs have only limited compatibility, and some polymer pairs have almost no compatibility. Therefore, the degree of compatibility can be divided into complete compatibility, partial compatibility and incompatibility.
[0066] The present invention uses a blended solution of a high modulus polymer 2 and a low modulus polymer 1 as a sheath solution, and a solution of an elastomeric polymer 1 as a core solution, and uses an electrostatic field direct writing method to prepare a polymer composite fiber membrane. Since a specific ratio of polymer 1 and polymer 2 electrostatic direct writing liquid (prepared by mixing two polymers in a certain mass ratio) is used, by controlling the ratio of the two solutes in the mixed direct writing liquid, the interfacial tension between the two polymers, the weak compatibility of the two (the interfacial tension is similar or the viscosity ratio is close to 1) and the phase separation effect are used to jointly drive the polymer 2 (such as polystyrene) to gradually form balls (that is, the effect of the interfacial tension causes the polymer 2 to stably exist in the form of micro / nano balls); thereby a polymer-based fiber membrane with a structure of "high modulus hemispherical polymer 2 dispersed on the surface of low modulus polymer 1 fiber" is prepared (that is, a fiber membrane formed by high modulus polymer 2 micron hemispheres dispersed in the elastomeric polymer 1 on the surface); the polymer fiber membrane with such a spherical micro-nano structure on the surface has differentiated performance due to the difference in the modulus of different areas on the surface due to the difference in material properties, and is called a heterogeneous structure fiber. In addition, due to the different interactions between the two polymers and the conductive fillers, there is also a significant difference in the dispersion concentration of conductive fillers such as conductive silver nanoparticles between the two polymers, which leads to the formation of an electrical heterostructure.
[0067] In addition, the present application can also regulate the shape of the micro-nano scale spheres formed by the dispersion of polymer 2 in polymer 1, such as spherical and ellipsoidal shapes, by controlling the phase separation process of polymer 2 and polymer 1 during the spinning process.
[0068] The embodiments given below are specific descriptions of the present invention. It is necessary to point out that the following embodiments are only used to further illustrate the present invention, and are not intended to limit the present invention in any form. Non-essential improvements and adjustments made by skilled persons in the field based on the above-mentioned contents of the present invention, such as changing the direct writing or spinning method or receiving method, the composition or concentration of the spinning solution, and the type of conductive nanomaterial and other simple processing methods or condition changes, still fall within the scope of protection of the present invention.
[0069] Embodiment 1:
[0070] A flexible and stretchable electronic material with a mechanical-electrical dual heterostructure based on a polymer-based fiber membrane, wherein the preparation method comprises the following steps:
[0071] 1) Prepare a styrene-butadiene copolymer solution: the mass fraction of SBS in toluene is 20%, and stir magnetically at room temperature for 8 hours until the SBS is completely dissolved.
[0072] 2) Prepare a mixed solution of SBS and PS: the mass ratio of SBS to PS is 9:1, the mass fraction of the solute in toluene is 20%, and magnetic stirring is performed at room temperature for 8 hours until the polymer is completely dissolved (the solution is transparent).
[0073] 3) Preparation of polymer-based fiber membrane by coaxial near-field electrostatic direct writing: add 3 mL of SBS solution in step 1) into the inner layer injection device and connect it to the inner layer (core layer) pipeline of the spinning needle; add 3 mL of SBS / PS mixed solution (mass ratio 9:1) in step 2) into the outer layer injection device and connect it to the outer layer (sheath layer) pipeline of the spinning needle; set the spinning parameters: propulsion speed: 2-3 mL / h; voltage: 4-6 kV; near-field electrostatic direct writing distance: 1-2 mm; obtain a polymer composite film; place the polymer composite film in a 40°C forced air drying oven and dry it for 3 h to remove the non-volatile solvent to obtain a polymer-based fiber membrane (denoted as SP91).
[0074] 4) Prepare a silver trifluoroacetate solution: the mass fraction of silver trifluoroacetate in ethanol solvent is 15%, and stir magnetically until it is completely transparent.
[0075] 5) Prepare a hydrazine hydrate mixed solution: slowly add hydrazine hydrate into a mixed solvent of water and ethanol in a volume ratio of 1:1:1.
[0076] 6) Preparation of elastomeric electronic fibers with uniformly distributed plastic micron dispersed phase (i.e., flexible and stretchable electronic materials with mechanical-electrical dual heterostructure): immersing the polymer-based fiber membrane obtained in step 3) into the silver trifluoroacetate solution obtained in step 4) for 30 minutes to adsorb silver ions in the solution; taking out and drying in the air for 5 minutes; then immersing the obtained polymer-based fiber membrane into the hydrazine hydrate mixed solution in step 5) to reduce the silver ions for 10 minutes, and the film gradually turns grayish white. After washing with a mixed solution of ethanol and water, it is dried to obtain a flexible and stretchable electronic material (denoted as SP91-Ag) in which a plastic micron dispersed phase with silver nanoparticles deposited is dispersed in SBS.
[0077] Example 1 Step 3) The fiber structure photo of SP91 obtained under an electron microscope is as follows Figure 1 As shown by Figure 1 It can be seen that when the polystyrene content in the sheath layer is low, the density of the dispersed phase formed in situ is low; but at this time it is already possible to ensure the construction of a heterogeneous structure of the plastic micron dispersed phase in the elastomer.
[0078] Embodiment 2:
[0079] A flexible and stretchable electronic material with a mechanical-electrical dual heterostructure based on a polymer-based fiber membrane, wherein the preparation method comprises the following steps:
[0080] 1) Prepare a styrene-butadiene copolymer solution: the mass fraction of SBS in toluene is 20%, and stir magnetically at room temperature for 8 hours until the SBS is completely dissolved.
[0081] 2) Prepare a mixed solution of SBS and PS: the mass ratio of SBS to PS is 8:2, the mass fraction of the solute in toluene is 20%, and magnetic stirring is performed at room temperature for 8 hours until the polymer is completely dissolved (the solution is transparent).
[0082] 3) Preparation of polymer-based fiber membrane by coaxial near-field electrostatic direct writing: add 3 mL of SBS solution in step (1) into the core layer injection device and connect it to the core layer pipeline of the spinning needle; add 3 mL of SBS / PS (mass ratio 8:2) mixed solution in step (2) into the sheath layer injection device and connect it to the sheath layer pipeline of the spinning needle; set the spinning parameters as follows: propulsion speed: 2-3 mL / h; voltage: 4-6 kV; near-field electrostatic direct writing distance: 1-2 mm; obtain a polymer composite film; place the polymer composite film in a 40°C forced air drying oven and dry it for 3 h to remove the non-volatile solvent, thereby obtaining a polymer-based fiber membrane (denoted as SP82).
[0083] 4) Prepare a silver trifluoroacetate solution: the mass fraction of silver trifluoroacetate in ethanol solvent is 15%, and stir magnetically until it is completely transparent.
[0084] 5) Prepare a hydrazine hydrate mixed solution: slowly add hydrazine hydrate into a mixed solvent of water and ethanol in a volume ratio of 1:1:1.
[0085] 6) Preparing a flexible and stretchable electronic material with a uniformly distributed plastic micron dispersed phase: immersing the fiber film obtained in step 3) into the silver trifluoroacetate solution obtained in step 4) for 30 minutes to adsorb the silver ions in the solution; taking it out and drying it in the air for 5 minutes; then immersing the obtained fiber film in the hydrazine hydrate mixed solution of step 5) to reduce the silver ions for 10 minutes, and the film gradually turns grayish white. After washing with a mixed solution of ethanol and water, it is dried to obtain an elastomeric electronic fiber modified with plastic nanospheres deposited with silver nanoparticles (i.e., a flexible and stretchable electronic material with a mechanical-electrical double heterostructure, denoted as SP82-Ag).
[0086] The fiber structure photo of SP82 obtained in Example 2 under an electron microscope is as follows Figure 2 As shown, after the polystyrene content increases, the size of the micron dispersed phase increases slightly compared with Example 1.
[0087] Embodiment three:
[0088] A flexible and stretchable electronic material with a mechanical-electrical dual heterostructure based on a polymer-based fiber membrane, wherein the preparation method comprises the following steps:
[0089] 1) Prepare a styrene-butadiene copolymer solution: the mass fraction of SBS in toluene is 20%, and stir magnetically at room temperature for 8 hours until the SBS is completely dissolved.
[0090] 2) Prepare a mixed solution of SBS and PS: the mass ratio of SBS to PS is 7:3, the mass fraction of the solute in toluene is 20%, and magnetic stirring is performed at room temperature for 8 hours until the polymer is completely dissolved (the solution is transparent).
[0091] 3) Preparation of polymer-based fiber membrane by coaxial near-field electrostatic direct writing: add 3 mL of SBS solution in step 1) into the core layer injection device and connect it to the core layer pipeline of the spinning needle; add 3 mL of SBS / PS (mass ratio 7:3) mixed solution in step 2) into the sheath layer injection device and connect it to the sheath layer pipeline of the spinning needle; set the spinning parameters: propulsion speed: 2-3 mL / h; voltage: 4-6 kV; near-field electrostatic direct writing distance: 1-2 mm; obtain a polymer composite film; place the film in a 40°C forced air drying oven and dry it for 3 h to remove the non-volatile solvent to obtain a polymer-based fiber membrane (denoted as SP73).
[0092] 4) Prepare a silver trifluoroacetate solution: the mass fraction of silver trifluoroacetate in ethanol solvent is 15%, and stir magnetically until it is completely transparent.
[0093] 5) Prepare a hydrazine hydrate mixed solution: slowly add hydrazine hydrate into a mixed solvent of water and ethanol in a volume ratio of 1:1:1.
[0094] 6) Preparing an elastomeric electronic fiber with a uniformly distributed plastic micron dispersed phase: immersing the fiber film obtained in step 3) into the silver trifluoroacetate solution obtained in step 4) for 30 minutes to adsorb the silver ions in the solution; taking it out and drying it in the air for 5 minutes; immersing the obtained fiber film into the hydrazine hydrate mixed solution of step 5) for 10 minutes to reduce the silver ions, and the film gradually turns grayish white. After washing with a mixed solution of ethanol and water, it is dried to obtain an elastomeric electronic fiber modified with plastic nanospheres with silver nanoparticles deposited (denoted as SP73-Ag).
[0095] The fiber structure photo of SP73 obtained in Example 3 under an electron microscope is as follows Figure 3 As shown by Figure 3 It can be seen that the size of the micron-sized PS dispersed phase increases significantly with the increase of PS content, but it has an excellent interface with the SBS matrix; this ensures the stability of the heterostructure and also shows the superiority of the method of using this system to prepare double heterostructure electronic thin films.
[0096] Embodiment 4:
[0097] A flexible and stretchable electronic material with a mechanical-electrical dual heterostructure based on a polymer-based fiber membrane, wherein the preparation method comprises the following steps:
[0098] 1) Prepare a styrene-butadiene copolymer solution: the mass fraction of SBS in toluene is 20%, and stir magnetically at room temperature for 8 hours until the SBS is completely dissolved.
[0099] 2) Prepare a mixed solution of SBS and PS: the mass ratio of SBS to PS is 6:4, the mass fraction of the solute in toluene is 20%, and magnetic stirring is performed at room temperature for 8 hours until the polymer is completely dissolved (the solution is transparent).
[0100] 3) Preparation of polymer-based fiber membrane by coaxial near-field electrostatic direct writing: Add 3 mL of SBS solution in step 1) into the core layer injection device and connect the core layer pipeline of the spinning needle; Add 3 mL of SBS / PS (mass ratio 6:4) mixed solution in step 2) into the sheath layer injection device and connect the sheath layer pipeline of the spinning needle; Set the spinning parameters: propulsion speed: 2-3 mL / h; voltage: 4-6 kV; near-field electrostatic direct writing distance: 1-2 mm; Get a polymer composite film. Place the film in a 40°C forced air drying oven for 3 hours to remove the non-volatile solvent, and get a polymer-based fiber membrane (denoted as SP64).
[0101] 4) Prepare a silver trifluoroacetate solution: the mass fraction of silver trifluoroacetate in ethanol solvent is 15%, and stir magnetically until it is completely transparent.
[0102] 5) Prepare a hydrazine hydrate mixed solution: slowly add hydrazine hydrate into a mixed solvent of water and ethanol in a volume ratio of 1:1:1.
[0103] 6) Preparing an elastomeric electronic fiber with a uniformly distributed plastic micron dispersed phase: immersing the fiber film obtained in step 3) into the silver trifluoroacetate solution obtained in step 4) for 30 minutes to adsorb the silver ions in the solution; taking it out and drying it in the air for 5 minutes; immersing the obtained fiber film into the hydrazine hydrate mixed solution of step 5) to reduce the silver ions for 10 minutes, and the film gradually turns grayish white. After washing with a mixed solution of ethanol and water, it is dried to obtain an elastomeric electronic fiber modified with plastic nanospheres with silver nanoparticles deposited (denoted as SP64-Ag).
[0104] The fiber structure photo of SP64 obtained in Example 4 under an electron microscope is as follows Figure 4 As shown in the figure, it can be seen that when the polystyrene content in the sheath layer is high, a larger PS dispersed phase has appeared on the fiber surface, indicating that this method can be used to regulate the degree of surface mechanical-electrical dual heterogeneity.
[0105] Embodiment five:
[0106] A flexible and stretchable electronic material with a mechanical-electrical dual heterostructure based on a polymer-based fiber membrane, wherein the preparation method comprises the following steps:
[0107] 1) Prepare a styrene-butadiene copolymer solution: the mass fraction of SBS in toluene is 20%, and stir magnetically at room temperature for 8 hours until the SBS is completely dissolved.
[0108] 2) Prepare a mixed solution of SBS and PS: the mass ratio of SBS to PS is 5:5, the mass fraction of the solute in toluene is 20%, and magnetic stirring is performed at room temperature for 8 hours until the polymer is completely dissolved (the solution is transparent).
[0109] 3) Preparation of polymer-based fiber membrane by coaxial near-field electrostatic direct writing: Add 3 mL of SBS solution in step 1) into the core layer injection device and connect the core layer pipeline of the spinning needle; Add 3 mL of SBS / PS (mass ratio 5:5) mixed solution in step 2) into the sheath layer injection device and connect the sheath layer pipeline of the spinning needle; Set the spinning parameters: propulsion speed: 2-3 mL / h; voltage: 4-6 kV; near-field electrostatic direct writing distance: 1-2 mm; Get a polymer composite film. Place the film in a 40°C forced air drying oven for 3 hours to remove the non-volatile solvent, and get a polymer-based fiber membrane (denoted as SP55).
[0110] 4) Prepare a silver trifluoroacetate solution: the mass fraction of silver trifluoroacetate in ethanol solvent is 15%, and stir magnetically until it is completely transparent.
[0111] 5) Prepare a hydrazine hydrate mixed solution: slowly add hydrazine hydrate into a mixed solvent of water and ethanol in a volume ratio of 1:1:1.
[0112] 6) Preparation of elastomeric electronic fibers with uniformly distributed plastic micron dispersed phase (i.e., flexible and stretchable electronic materials with mechanical-electrical double heterostructure): immersing the fiber film obtained in step 3) into the silver trifluoroacetate solution obtained in step 4) for 30 minutes to adsorb silver ions in the solution; taking out and drying in air for 5 minutes; immersing the obtained fiber film into the mixed solution of hydrazine hydrate in step 5) to reduce the silver ions for 10 minutes, and the film gradually turns grayish white. After washing with a mixed solution of ethanol and water, drying is performed to obtain elastomeric electronic fibers modified with plastic nanospheres with deposited silver nanoparticles (i.e., flexible and stretchable electronic materials with mechanical-electrical double heterostructure, denoted as SP55-Ag).
[0113] Example 5 The fiber structure photo of SP55 obtained under an electron microscope is as follows Figure 5 As shown in the figure, it can be seen that when the sheath polystyrene content is equal to the SBS content, the PS dispersed phase on the surface still remains relatively uniform and has a higher density.
[0114] Comparative Example 1:
[0115] 1) Prepare a solution of thermoplastic styrene-butadiene copolymer: the mass fraction of styrene-butadiene copolymer in solvent (xylene) is 20%, and stir magnetically until the solution becomes transparent.
[0116] 2) Preparation of polymer-based fiber membrane by coaxial near-field electrostatic direct writing: 3 mL of styrene-butadiene copolymer solution in step (1) was added to the injection device and connected to the needle pipeline; the electrostatic direct writing parameters were set as follows: propulsion speed: 2-3 mL / h; voltage: 4-6 kV; distance between the needle and the receiving plate: 1-2 mm) to obtain a styrene-butadiene copolymer fiber film; the fiber film was placed in a 40°C forced air drying oven and dried for 3 h to remove the non-volatile solvent, thereby obtaining a fiber film (denoted as SBS).
[0117] 3) Prepare a silver trifluoroacetate solution: the mass fraction of silver trifluoroacetate in ethanol solvent is 15%, and stir magnetically until it is completely transparent.
[0118] 4) Prepare a hydrazine hydrate mixed solution: slowly add hydrazine hydrate into a mixed solvent of water and ethanol in a volume ratio of 1:1:1.
[0119] 5) Preparation of elastomeric electronic fibers: Immerse the fiber film obtained in step 2) in the silver trifluoroacetate solution obtained in step 3) for 30 minutes to absorb the silver ions in the solution; take it out and dry it in the air for 5 minutes. Immerse the obtained fiber film in the mixed solution of hydrazine hydrate in step 4) to reduce the silver ions, and the film gradually turns grayish white. After washing with a mixed solution of ethanol and water, it is dried to obtain an elastomeric electronic fiber with silver nanoparticles deposited (referred to as SBS-Ag).
[0120] Comparative Example 2:
[0121] 1) Prepare a styrene-butadiene copolymer solution: the mass fraction of SBS in toluene is 20%, and stir magnetically at room temperature for 8 hours until the SBS is completely dissolved.
[0122] 2) Prepare a mixed solution of SBS and PS: the mass ratio of SBS to PS is 4:6, the mass fraction of the solute in toluene is 20%, and magnetic stirring is performed at room temperature for 8 hours until the polymer is completely dissolved (the solution is transparent).
[0123] 3) Preparation of polymer-based fiber membrane by coaxial near-field electrostatic direct writing: Add 3 mL of SBS solution in step 1) into the core layer injection device and connect the core layer pipeline of the spinning needle; Add 3 mL of SBS / PS (mass ratio 4:6) mixed solution in step 2) into the sheath layer injection device and connect the sheath layer pipeline of the spinning needle; Set spinning parameters: propulsion speed: 2-3 mL / h; voltage: 4-6 kV; near-field electrostatic direct writing distance: 1-2 mm; Get polymer composite film. Place the film in a 40°C forced air drying oven for 3 hours to remove the non-volatile solvent, and get a polymer-based fiber membrane (denoted as SP46).
[0124] 4) Prepare a silver trifluoroacetate solution: the mass fraction of silver trifluoroacetate in ethanol solvent is 15%, and stir magnetically until it is completely transparent.
[0125] 5) Prepare a hydrazine hydrate mixed solution: slowly add hydrazine hydrate into a mixed solvent of water and ethanol in a volume ratio of 1:1:1.
[0126] 6) Preparing an elastomeric electronic fiber with a uniformly distributed plastic micron dispersed phase: immersing the fiber film obtained in step 3) into the silver trifluoroacetate solution obtained in step 4) for 30 minutes to adsorb the silver ions in the solution; taking it out and drying it in the air for 5 minutes; immersing the obtained fiber film into the hydrazine hydrate mixed solution of step 5) for 10 minutes to reduce the silver ions, and the film gradually turns grayish white. After washing with a mixed solution of ethanol and water, it is dried to obtain an elastomeric electronic fiber modified with plastic nanospheres with silver nanoparticles deposited (denoted as SP46-Ag).
[0127] The fiber structure photo of SP46 obtained in Comparative Example 2 under an electron microscope is as follows Figure 7 As shown, when the sheath polystyrene content exceeds the SBS content, an obvious phase reversal has occurred.
[0128] The samples obtained from the embodiments and comparative examples were subjected to the following tests:
[0129] Mechanical properties test: The SP double heterogeneous composite film samples were tested at room temperature using a universal testing machine (Instron 5967); the tensile rate was 50 mm / min.
[0130] Electrical performance test: Use the two-probe method to test, fix the length of the sample and load voltage at both ends. The resistance meter (Keithley 2400) can read the resistance, and the conductivity is calculated from the resistance value and the geometric dimensions of the sample.
[0131] The sample was stretched using a self-made stretching platform, and a digital source meter (Keithley 2400) was used to record the electrical signal during the strain process (two-electrode method), where the test loading voltage of the sensor was 1V.
[0132] The fiber structure photo of SBS obtained in Comparative Example 1 under an electron microscope is as follows: Figure 6 As shown in the figure, it can be seen that the surface of the styrene-butadiene copolymer fiber membrane is smooth and the structure is uniform, which means that it is impossible to construct a micro-nanoscale heterogeneous structure on the fiber of the present invention through a single component design under the same electrostatic direct writing conditions.
[0133] The SEM of the silver nanoparticle conductive layer generated in situ in Example 4 of the present invention is as follows Figure 8 As shown in the figure, it can be seen that a large amount of silver nanoparticles are loaded on both phases of the membrane surface, and the content of silver nanoparticles in the two phases shows obvious differences. Fig. 9 The difference in modulus and conductivity of SBS and PS after loading silver nanoparticles is two orders of magnitude (10 2 ), indicating that the method of the present invention successfully constructs a surface force-electric dual heterostructure. In addition, the PS dispersed phase sizes of Examples 1 to 5 are statistically analyzed, such as Fig.10 As shown, it can be seen that with the increase of PS content in the sheath, the size of the PS dispersed phase shows a trend of first increasing and then decreasing, which is conducive to the regulation of the mechanical-electrical dual heterostructure.
[0134] Fig.11 The figure shows the comparison between the strain sensing performance (dependence between relative resistance change and strain) of the electronic fiber materials (SP91, SP28, SP37, SP46, SP55, SBS and SP64) obtained in Examples 1 to 5, Comparative Example 1 and Comparative Example 2; Fig.11 It can be seen that the composite material elastomeric electronic fiber of the plastic in the form of microsphere dispersed phase dispersed in the elastomeric fiber of the present invention has excellent, linear response and stable relative resistance-strain change characteristics in a wide strain (up to 0-70%) loading range; while in the patent application with publication number CN113818236A, the strain range of the stretched electronic material with a modulus heterogeneous structure is up to 25%, such as Fig.12 This is because the heterogeneous structure of rigid polystyrene microspheres dispersed on the SBS surface can change the local stress distribution, and together with the heterogeneous electrical properties, it inhibits the penetrating destruction of the structural change of the conductive path during strain loading, thereby slowing down the speed of the resistance mutation or reducing the degree of this mutation. The SBS elastomer fiber without heterogeneous structure shown in Comparative Example 1 cannot maintain stable sensitivity under low strain and exhibits typical nonlinear resistance-strain response characteristics. This is because the uniform fiber surface cannot inhibit the rapid destruction of the silver conductive layer during the stretching process, that is, the penetrating diffusion of the crack.
[0135] The method of the present invention is not limited to polystyrene and styrene-butadiene copolymers, and the conductive filler is not limited to Ag. The type of elastomeric fiber, the high modulus plastic phase, and the conductive filler can be selected as needed to achieve modulus difference and modulus gradient, as well as the geometric shape and size, continuous design and construction of electrically heterogeneous structures, providing a new idea for preparing heterogeneous structural elastomeric fibers or films with linear high-sensitivity resistance-strain response in a wide strain range.
[0136] Although the present invention has been described above in conjunction with the embodiments, it will be apparent to those skilled in the art that various modifications may be made to the embodiments without departing from the spirit and scope of the claims.
Claims
1. A flexible and stretchable electronic material, characterized in that: The flexible and stretchable electronic material is a conductive material deposited on the surface of a polymer-based fiber membrane; the polymer-based fiber membrane is prepared by spinning a first solution as a core layer solution and a second solution as a sheath layer solution, the first solution is a solution containing polymer 1, the second solution is a solution containing polymer 1 and polymer 2, and the mass ratio of polymer 1 to polymer 2 in the second solution is 9:1 to 5:5; Wherein, the polymer 1 and polymer 2 are partially compatible in thermodynamics, the interactions between the polymer 1 and polymer 2 and the conductive material are different, and the Young's modulus of polymer 2 is greater than that of polymer 1; and, the polymer 1 is a thermoplastic elastomer, and the polymer 2 is a thermoplastic plastic; the polymer 1 is selected from: thermoplastic polystyrene-butadiene-styrene block copolymer, styrene-ethylene-butadiene-styrene block copolymer or styrene-isoprene-styrene triblock copolymer; the polymer 2 is selected from: polystyrene, acrylonitrile-butadiene-styrene copolymer, styrene-acrylonitrile copolymer or polypropylene.
2. A flexible and stretchable electronic material according to claim 1, characterized in that: The mass ratio of polymer 1 to polymer 2 in the second solution is 8:2 to 5:
5.
3. A flexible and stretchable electronic material according to any one of claims 1-2, characterized in that: The different interactions between the polymer 1 and the polymer 2 and the conductive material refer to: different physical interactions or different chemical interactions between the polymer 1 and the conductive material; wherein the physical interaction refers to: conjugated π electron-ion, π-π conjugation or van der Waals force.
4. A flexible and stretchable electronic material according to any one of claims 1-2, characterized in that: In the flexible stretchable electronic material, the ratio of the electrical conductivity of polymer 1 after the conductive material is deposited on the surface to the electrical conductivity of polymer 2 after the conductive material is deposited on the surface is ≥10.
5. A flexible and stretchable electronic material according to any one of claims 1-2, characterized in that: The Young's modulus of polymer 1 and polymer 2 satisfy that the ratio of the Young's modulus of polymer 2 to the Young's modulus of polymer 1 is not less than 100.
6. A flexible and stretchable electronic material according to any one of claims 1-2, characterized in that: The polymer 1 and polymer 2 are selected from the following combinations: thermoplastic polystyrene-butadiene-styrene block copolymer and polypropylene, thermoplastic polystyrene-butadiene-styrene block copolymer and acrylonitrile-butadiene-styrene copolymer, thermoplastic polystyrene-butadiene-styrene block copolymer and styrene-acrylonitrile copolymer, styrene-isoprene-styrene triblock copolymer and polystyrene, or styrene-isoprene-styrene triblock copolymer and styrene-acrylonitrile copolymer.
7. A flexible and stretchable electronic material according to any one of claims 1-2, characterized in that: The conductive material is metal nanoparticles or nanowires, one-dimensional or two-dimensional carbon-based conductive materials, or conductive polymers.
8. The flexible and stretchable electronic material according to claim 7, characterized in that: The metal in the metal nanoparticles or nanowires is silver, gold or copper.
9. A flexible and stretchable electronic material according to any one of claims 1-2, characterized in that: The spinning method is a coaxial near-field electrostatic direct writing method or a wet spinning method.
10. A flexible and stretchable electronic material according to any one of claims 1-2, characterized in that: The solvents of the first solution and the second solution are selected from: a mixed solvent of toluene and ethylene dichloride, toluene or ethylene dichloride.
11. A flexible and stretchable electronic material according to any one of claims 1-2, characterized in that: The mass concentration of the first solution is 15-25%.
12. A flexible and stretchable electronic material according to any one of claims 1-2, characterized in that: The mass concentration of the second solution is 10-25%.
13. The method for preparing the flexible and stretchable electronic material according to any one of claims 1 to 12, characterized in that: The preparation method comprises: depositing a conductive material on the surface of the polymer-based fiber membrane.
14. Use of a flexible stretchable electronic material in the preparation of a flexible stretchable strain sensing material or a strain sensor, wherein the flexible stretchable electronic material is a flexible stretchable electronic material according to any one of claims 1 to 12 or a material prepared by the preparation method according to claim 13.
15. A method for preparing a polymer-based fiber membrane, characterized in that: The preparation method comprises: using the first solution as the core layer solution and the second solution as the sheath layer solution through a spinning method; The first solution is a solution containing only polymer 1, and the second solution is a solution containing polymer 1 and polymer 2, and the mass ratio of polymer 1 to polymer 2 in the second solution is 9:1 to 5:5; Wherein, the polymer 1 and polymer 2 are partially compatible in thermodynamics, and the Young's modulus of polymer 2 is greater than that of polymer 1; and, the polymer 1 is a thermoplastic elastomer, and the polymer 2 is a thermoplastic plastic; the polymer 1 is selected from: thermoplastic polystyrene-butadiene-styrene block copolymer, styrene-ethylene-butadiene-styrene block copolymer or styrene-isoprene-styrene triblock copolymer; the polymer 2 is selected from: polystyrene, acrylonitrile-butadiene-styrene copolymer, styrene-acrylonitrile copolymer or polypropylene.
16. The method for preparing a polymer-based fiber membrane according to claim 15, characterized in that: The mass ratio of polymer 1 to polymer 2 in the second solution is 8:2 to 5:
5.
17. A method for preparing a polymer-based fiber membrane according to any one of claims 15-16, characterized in that: The Young's modulus of polymer 1 and polymer 2 satisfy that the ratio of the Young's modulus of polymer 2 to the Young's modulus of polymer 1 is not less than 100.
18. A method for preparing a polymer-based fiber membrane according to any one of claims 15-16, characterized in that: The polymer 1 and polymer 2 are selected from the following combinations: thermoplastic polystyrene-butadiene-styrene block copolymer and polypropylene, thermoplastic polystyrene-butadiene-styrene block copolymer and acrylonitrile-butadiene-styrene copolymer, thermoplastic polystyrene-butadiene-styrene block copolymer and styrene-acrylonitrile copolymer, styrene-isoprene-styrene triblock copolymer and polystyrene, or styrene-isoprene-styrene triblock copolymer and styrene-acrylonitrile copolymer.
19. A method for preparing a polymer-based fiber membrane according to any one of claims 15-16, characterized in that: The microstructural feature of the polymer-based fiber membrane is that polymer 2 is distributed in the polymer 1 matrix as a dispersed phase.
20. A method for preparing a polymer-based fiber membrane according to any one of claims 15-16, characterized in that: The spinning method is a coaxial near-field electrostatic direct writing method or a wet spinning method.
21. A method for preparing a polymer-based fiber membrane according to any one of claims 15-16, characterized in that: The spinning method is a coaxial near-field electrostatic direct writing method. During the coaxial near-field electrostatic direct writing process, the core-sheath layer spinning solution advancing speed is 1-10 mL / h; the voltage is 3-10 kV; and the near-field electrostatic direct writing distance is 1-2 mm.
22. A method for preparing a polymer-based fiber membrane according to any one of claims 15-16, characterized in that: The solvents of the first solution and the second solution are selected from: a mixed solvent of toluene and ethylene dichloride, toluene or ethylene dichloride.
23. A method for preparing a polymer-based fiber membrane according to any one of claims 15-16, characterized in that: The mass concentration of the first solution is 15-25%.
24. A method for preparing a polymer-based fiber membrane according to any one of claims 15-16, characterized in that: The mass concentration of the second solution is 10-25%.
25. A polymer-based fiber membrane, prepared by the method according to any one of claims 15 to 24.
26. Use of a polymer-based fiber membrane in preparing a flexible and stretchable electronic material, wherein the polymer-based fiber membrane is prepared by the method according to any one of claims 15 to 24.