Preparation method of NASICON composite electrolyte with sandwich structure and sodium ion battery application research of NASICON composite electrolyte

By introducing PVDF and SbF3 layers on both sides of the NASICON electrolyte material to form a sandwich structure, the problem of poor contact between NASICON electrolyte and electrode is solved, the electrochemical performance and cycle stability of sodium ion batteries are significantly improved, and the safety of the batteries is enhanced. sex.

CN119009078AInactive Publication Date: 2024-11-22GUANGDONG UNIV OF TECH

Patent Information

Application Number
CN202411090665.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The poor interface contact and compatibility between NASICON solid electrolyte and electrode leads to poor electrochemical performance, especially the problems of metal dendrites' growth and large interface resistance, which affects the cycling performance of sodium ion batteries.

Method used

Using the NASICON composite electrolyte material in the sandwich structure, the polymer layer PVDF and the inorganic layer SbF3 are introduced on both sides of the NASICON oxide ceramic sheet, and prepared by high-temperature solid-phase synthesis method and solution drop coating method to form a sandwich structure to improve interface compatibility. Sex and stability.

Benefits of technology

It significantly improves the electrochemical performance of sodium ion batteries, including rate performance and cycle stability, reduces the growth of sodium dendrites, and enhances the safety and capacity retention of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119009078A_ABST
    Figure CN119009078A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of sodium-ion battery materials, and particularly relates to a preparation method of a sandwich structure NASICON composite electrolyte and application research of the sandwich structure NASICON composite electrolyte on a sodium-ion battery, and the preparation method of the sandwich structure NASICON composite electrolyte can comprise the following steps: preparing an NASICON electrolyte sheet by a high-temperature solid-phase method, and then preparing the sandwich structure NASICON composite electrolyte sheet by a solution dispensing method. An AB3 layer is introduced to one side of the NASICON electrolyte in contact with the Na metal negative electrode, the A element is one or more of Bi, Sb and Sn, and the B element is one or more of I, Br and F. And meanwhile, a polymer layer is introduced to one side of the NASICON electrolyte in contact with the positive electrode, so that the final NASICON composite electrolyte with the sandwich structure is obtained. According to the NASICON composite electrolyte with the sandwich structure, the electrochemical performance of a sodium ion battery is effectively improved, a gap between the NASICON and sodium metal can be filled with the AB3 modification layer, the wettability of the NASICON on the sodium metal is effectively improved, and growth of sodium dendrites is inhibited. And secondly, by utilizing the flexibility and interface contact property of the polymer layer, the problems of poor solid-solid interface contact and deterioration of interface contact caused by volume expansion of the positive electrode active material in the charging and discharging process are relieved. And due to the synergistic effect of the two, the prepared NASICON composite electrolyte with the sandwich structure shows high specific capacity and excellent capacity retention ratio and cycling stability in the sodium-ion battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of new energy battery materials, and more specifically, to a preparation method of a sandwich structure NASICON composite electrolyte and research on its application in sodium ion batteries. Background Art

[0002] Na and Li belong to the same main group and have similar electrochemical properties. In addition, the abundant sodium resources on earth and the low production cost make sodium-ion batteries (SIBs) an ideal alternative to lithium-ion batteries. However, similar to lithium-ion batteries (LIBs), when using traditional organic liquid electrolytes to match SIBs, there are safety issues caused by the reaction between flammable organic electrolytes and active sodium metals. The most prominent problem is the growth of sodium dendrites, which may cause short circuits or even explosions of SIBs. The safety issues in the use of liquid batteries can be alleviated to a certain extent by adding flame retardants, developing high-temperature resistant diaphragms, surface modification of positive and negative electrode materials, optimizing the design of battery structure, and improving the cooling system. However, it cannot ensure the safe and efficient long-term operation of large-capacity and high-power battery systems. Therefore, the use of inorganic solid electrolytes can effectively eliminate the various troubles brought by traditional liquid organic electrolytes, making the battery safer and having a longer cycle life, thereby realizing high-energy density and high-safety sodium metal batteries.

[0003] At present, the most promising ceramic electrolyte types are Na-β-A12O3, perovskite structure, Garnet structure and NASICON structure oxide electrolyte. 1+x Al x Ti 2-x (PO4)3,Na 1+ x Zr2Si x P 3-x O 12 ) has stable chemical properties, a wide electrochemical window and relatively high ionic conductivity (up to 10 at room temperature). -3 S cm -1), but due to the complex interface contact state with the solid metal electrode, it is easy to produce problems such as large interface contact resistance and metal dendrite growth, resulting in poor cycle performance of the resulting solid metal battery. In order to solve the problems of poor electrochemical performance caused by large interface resistance and metal dendrite growth of NASICON solid electrolyte, researchers have developed a variety of strategies, such as doping and modifying the electrolyte, surface coating of the positive electrode material, and optimizing the synthesis method of the electrolyte. However, there are still problems such as poor physical contact and compatibility of the solid-solid interface between the NASICON inorganic electrolyte and the electrode. Therefore, it is necessary to design a NASICON composite electrolyte material with a simple preparation method and excellent performance.

[0004] Application Contents

[0005] In order to overcome at least one problem existing in the prior art, the primary purpose of the present application is to provide a sandwich structure NASICON composite electrolyte material.

[0006] The second objective of the present application is to provide a method for preparing the above-mentioned sandwich structure NASICON composite electrolyte material.

[0007] The third purpose of the present application is to provide the application of the sandwich structure NASICON composite electrolyte. The sandwich structure NASICON composite electrolyte of the present application exhibits good electrochemical performance after being applied to sodium ion batteries, and has the advantages of high safety, good interface compatibility, excellent cycle stability, etc.

[0008] To achieve the above objectives, this application provides the following solutions:

[0009] The present application provides a sandwich structure NASICON composite electrolyte material, and the NASICON type oxide ceramic is obtained by high temperature solid phase synthesis as a matrix. Wherein, a polymer layer PVDF and an inorganic layer AB3 are introduced on both sides of the NASICON type oxide ceramic sheet, wherein A is one or more of Bi, Sb and Sn, and B is one or more of I, Br and F, and the sandwich structure NASICON composite electrolyte material has good interface compatibility with the positive and negative electrodes.

[0010] The present application also provides a method for preparing the above-mentioned sandwich structure NASICON composite electrolyte material, comprising the following steps:

[0011] S1. Na2CO3, ZrO2, SiO2 and NH4H2PO4 were weighed in a stoichiometric ratio, dispersed in anhydrous ethanol, ball-milled, pressed and sintered, and finally polished to obtain a pure NASICON electrolyte sheet;

[0012] S2. The SbF3 powder was dissolved in ethylene glycol dimethyl ether and stirred to obtain a SbF3 precursor solution, and PVDF and NaTFSI were dissolved in N,N-dimethylformamide and stirred to obtain a PVDF precursor solution;

[0013] S3. The SbF3 precursor solution is added dropwise to one side of the NASICON electrolyte sheet to obtain the SbF3-NASICON electrolyte, and the PVDF precursor solution is added dropwise to the other side of the SbF3-NASICON electrolyte to obtain the PVDF-NZSP-SbF3 electrolyte.

[0014] Further technical solution of the present application: The preparation of the NASICON substrate in step S1 specifically includes the following steps:

[0015] S11. Weigh Na2CO3, ZrO2, SiO2 and NH4H2PO4 according to the stoichiometric ratio, and then disperse them in anhydrous ethanol and ball mill for 12 hours.

[0016] S12. After ball milling, pour the solution into a watch glass and transfer to an oven to dry at 80°C for 12 hours to remove ethanol. The dried powder is then sintered at 1000°C for 12 hours. The sintered powder is then ground, ball milled and dried in the same conditions as above.

[0017] S13. The dried powder was pressed into a disc with a diameter of 15 mm and sintered at 1200°C for 10 h to obtain a NASICON electrolyte sheet.

[0018] S14. Finally, the NASICON electrolyte sheet is polished by a grinding and polishing machine.

[0019] A further technical solution of the present application: the Na2CO3 and NH4H2PO4 described in step S11 should be appropriately excessive.

[0020] A further technical solution of the present application: the rotation speed of the ball mill described in step S11 is set to 400 rpm.

[0021] Further technical solution of the present application: the powder obtained after sintering in step S12 should be ground as finely as possible. The ball milling time is still 12 hours, and the drying condition is still 80° C. for 12 hours.

[0022] A further technical solution of the present application: In step S13, the pressure needs to be increased to 15 MPa to 20 MPa.

[0023] Further technical solution of the present application: the grits of sandpaper used for grinding and polishing in step S14 are: 240, 400, 2000, 4000, 5000 grit respectively.

[0024] Further technical solution of the present application: The preparation of the SbF3 and PVDF precursor solution in step S2 specifically includes the following steps:

[0025] S21.SbF3 precursor solution preparation:

[0026] The SbF3 powder was dissolved in ethylene glycol dimethyl ether (DME) and stirred at room temperature for 12 h to obtain a SbF3 precursor solution.

[0027] S22. Preparation of PVDF precursor solution:

[0028] PVDF and NaTFSI were dissolved in N,N-dimethylformamide (DMF) and stirred at 60° C. for 12 h to obtain a PVDF precursor solution.

[0029] Further technical solution of the present application: The mass of the SbF3 powder and DME in step S21 is (0.1 g: 10 mL).

[0030] A further technical solution of the present application: The masses of PVDF, NaTFSI and DMF in step S22 are (0.25 g: 0.1 g: 7 mL).

[0031] Further technical solution of the present application: The experimental operations described in steps S21 and S22 are all carried out in a glove box under an Ar gas atmosphere with H2O<0.1, O2<0.1.

[0032] Further technical solutions of the present application: Step S3 The preparation of the sandwich structure PVDF-NZSP-SbF3 composite electrolyte specifically includes the following steps:

[0033] S31. Add the SbF3 precursor solution dropwise to one side of the NASICON electrolyte sheet, place it on a constant temperature heating table at 60°C and heat it for 3 hours to obtain the SbF3-NASICON electrolyte.

[0034] S32. Add the PVDF precursor solution dropwise to the other side of the electrolyte sheet, place it on a constant temperature heating table at 60°C and heat it for 3 hours to obtain PVDF-NZSP-SbF3 electrolyte.

[0035] S33. Add the SbF3 precursor solution dropwise to the other side of the NASICON electrolyte sheet, place it on a constant temperature heating table at 60°C and heat it for 3 hours to obtain SbF3-NASICON-SbF3 electrolyte.

[0036] A further technical solution of the present application: In steps S31 and S33, the amount of SbF3 precursor solution added is 50 μL and is evenly coated.

[0037] A further technical solution of the present application: In step S32, the amount of the PVDF precursor solution added is 60 μL, and it is evenly coated.

[0038] A further technical solution of the present application: the coating process in step S3 is carried out under an Ar gas atmosphere.

[0039] The present application also provides a sodium ion battery, which comprises the sandwich structure NASICON composite electrolyte material according to claim 1.

[0040] The present application also provides a method for preparing the above-mentioned sodium ion battery, comprising the following steps:

[0041] S1 '. The sandwich structure NASICON composite electrolyte sheet according to claim 1 is dried and sealed.

[0042] S2'. In a water-free and oxygen-free glove box, place the positive electrode shell of the sodium ion battery with the opening facing upwards and lay it flat on a pad, place the positive electrode sheet in the center of the positive electrode shell, then drip the electrolyte to wet the surface of the electrode sheet, and place the electrolyte sheet of step S32 in the center of the electrode sheet; clamp the sodium metal sheet and place it in the center of the electrolyte sheet; finally, place the gasket and the spring in the center of the sodium metal sheet, cover the negative electrode shell and seal it to obtain a sodium ion battery.

[0043] Furthermore, the electrolyte used is sodium perchlorate solution (1M NaClO4 in EC / EMC (1:1) + 5% FEC), and the positive electrode used is Na3V2(PO4)3 or NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2.

[0044] Compared with the prior art, the beneficial effects of this application are:

[0045] The present application discloses a method for preparing a sandwich structure NASICON composite electrolyte material. A NASICON matrix is ​​obtained by a simple high-temperature solid-phase synthesis method, and a sandwich structure NASICON composite electrolyte is obtained by drying using a simple solution drop coating method.

[0046] The sandwich structure NASICON composite electrolyte of the present application shows good electrochemical performance after being applied to sodium ion batteries, and has the advantages of high safety, good interface compatibility, excellent cycle stability, etc., as shown in the following:

[0047] First, through the in-situ conversion reaction between SbF3 and sodium metal, a Na xThe ion-electron composite conductive layer composed of Sb alloy and NaF effectively improves the diffusion and conduction of ions at the interface, promotes the uniform deposition of sodium, and can significantly promote ion migration and improve interface stability, significantly improving the rate performance and cycle stability of sodium ion batteries.

[0048] Secondly, a PVDF polymer layer was introduced on the side of the NASICON electrolyte in contact with the positive electrode. Figure 3 From the cross-sectional SEM image of PVDF-NZSP, we can see that there is a 2μm thick PVDF coating on the surface of the NASICON electrolyte sheet. Since PVDF polymer has a certain ductility, it can alleviate the problems of poor solid-solid interface contact and deterioration of interface contact caused by the volume expansion of the positive electrode active material during charging and discharging.

[0049] In the third aspect, the PVDF-NZSP-SbF3 composite electrolyte material is applied to the preparation of a sodium ion battery, which is made of an electrode sheet, a sodium metal sheet, an electrolyte sheet, a spring, a gasket, and a positive and negative electrode shell. The sodium ion battery prepared by the NASICON composite electrolyte material used in this application has excellent electrochemical performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0050] Figure 1 This is a flow chart of the preparation method of the sandwich structure NASICON composite electrolyte of the present application.

[0051] Figure 2 These are SEM and TEM images of the surface of the NASICON composite electrolyte sheet prepared in this application.

[0052] Figure 3 These are the SEM and TEM images of the cross-section of the NASICON composite electrolyte prepared in this application.

[0053] Figure 4 (a) XRD pattern of SbF3-NZSP electrolyte of NASICON composite electrolyte material prepared in this application.

[0054] Figure 4 (b) XRD pattern of PVDF-NZSP electrolyte of NASICON composite electrolyte material prepared in this application.

[0055] Figure 5 (a) is an AFM image of the surface of the NASICON matrix electrolyte sheet prepared in this application.

[0056] Figure 5 (b) AFM image of the surface of the NASICON composite electrolyte sheet prepared in this application.

[0057] Figure 6Room temperature AC impedance spectra of the NASICON composite electrolyte material and the NASICON matrix electrolyte material prepared in this application.

[0058] Figure 7 (a) is a critical current density test diagram of the Na symmetric battery of the NASICON matrix electrolyte material prepared in this application at room temperature.

[0059] Figure 7 (b) is a critical current density test diagram of the Na symmetric battery of the NASICON composite electrolyte material prepared in this application at room temperature.

[0060] Figure 8 This is a comparison chart of the cycling performance of the NASICON composite electrolyte material and the NASICON matrix electrolyte material prepared in this application as sodium ion battery electrolytes at a current density of 0.2C.

[0061] Fig. 9 This is the cycling performance diagram of the NASICON composite electrolyte material prepared in this application at a current density of 2C.

[0062] Fig.10 This is a rate performance diagram of the NASICON composite electrolyte material prepared in this application as a sodium ion battery electrolyte. DETAILED DESCRIPTION

[0063] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. In the examples, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0064] It should be noted that:

[0065] In this application, unless otherwise specified, all the embodiments and preferred implementation methods mentioned herein can be combined with each other to form a new technical solution.

[0066] In the present application, unless otherwise specified, each reaction or operation step can be carried out sequentially or in a sequential manner. Preferably, the reaction method herein is carried out sequentially.

[0067] Unless otherwise specified, the professional and scientific terms used herein are the same as those familiar to those skilled in the art. In addition, any method or material similar or equivalent to the described content may also be applied to the present application.

[0068] Explanation of terms

[0069] NZSP: Na3Zr2Si2PO 12 Abbreviation for electrolyte material;

[0070] PVDF: polyvinylidene fluoride;

[0071] SEM: scanning electron microscope;

[0072] TEM: transmission electron microscope;

[0073] AFM: atomic force microscope;

[0074] The present application provides a sandwich structure NASICON composite electrolyte material, which is based on NASICON-type oxide ceramics. A polymer layer PVDF and an inorganic layer AB3 are introduced on both sides of the NASICON-type oxide ceramic sheet, respectively, wherein A is one or more of Bi, Sb and Sn, and B is one or more of I, Br and F, and the sandwich structure NASICON composite electrolyte material has good interface compatibility with the positive and negative electrodes.

[0075] In some preferred embodiments of the present application, the above-mentioned inorganic layer is SbF3.

[0076] This application cleverly uses NASICON electrolyte as a matrix, and coats SbF3 and PVDF on both sides of the NASICON electrolyte sheet by a simple solution drop coating method. After drop coating, a modified layer uniformly distributed on the surface of the electrolyte sheet is synthesized by drying under relatively mild conditions (60°C, Ar). At the same time, the PVDF-NZSP-SbF3 material is used as a sodium ion battery electrolyte, and excellent electrochemical performance (excellent cycle performance and rate performance) is obtained.

[0077] In terms of cycle performance, at a current density of 0.2C, the capacity retention rate can still be as high as 92.17% after 720 cycles. At a high current density of 2C, it can cycle more than 450 times and maintain a high reversible specific capacity and capacity retention rate. In terms of rate performance, even at a current density of 2C, the battery can work normally and obtain 90.2mAh g -1 The reversible specific capacity and sodium storage capacity of PVDF-NZSP-SbF3 are significantly better than those of NASICON electrolyte matrix, and thus it has important applications in sodium ion batteries.

[0078] On the other hand, the present application provides a method for preparing the above-mentioned sandwich structure NASICON composite electrolyte material, comprising the following steps:

[0079] S1. Na2CO3, ZrO2, SiO2 and NH4H2PO4 were weighed in a stoichiometric ratio, dispersed in anhydrous ethanol, ball-milled, pressed and sintered, and finally polished to obtain a pure NASICON electrolyte sheet;

[0080] S2. The SbF3 powder was dissolved in ethylene glycol dimethyl ether and stirred to obtain a SbF3 precursor solution, and PVDF and NaTFSI were dissolved in N,N-dimethylformamide and stirred to obtain a PVDF precursor solution;

[0081] S3. The SbF3 precursor solution is added dropwise to one side of the NASICON electrolyte sheet to obtain the SbF3-NASICON electrolyte, and the PVDF precursor solution is added dropwise to the other side of the SbF3-NASICON electrolyte to obtain the PVDF-NZSP-SbF3 electrolyte.

[0082] In some preferred embodiments, the Na2CO3 and NH4H2PO4 are in appropriate excess, and the excess of Na2CO3 and NH4H2PO4 is about 10-15%.

[0083] In some preferred embodiments, the entire experimental operation of step S2 is performed in a glove box under an Ar gas atmosphere with H2O<0.1, O2<0.1.

[0084] In some preferred embodiments, in step S1, the ball milling time is 12 hours, and the sintering temperature is 1000° C. for 12 hours.

[0085] In some preferred embodiments, in step S2, the stirring time is 12 hours.

[0086] In some preferred embodiments, in step S3, the amount of the SbF3 precursor solution added is 50 μL, and the amount of the PVDF precursor solution added is 60 μL.

[0087] In some preferred embodiments, in step S3, the inert gas is an argon atmosphere.

[0088] The present application also provides a sodium ion battery, in which the electrolyte is the above-mentioned sandwich structure NASICON composite electrolyte material.

[0089] On the other hand, the present application provides a method for preparing the above-mentioned sodium ion battery, comprising the following steps:

[0090] S1 '. The sandwich structure NASICON composite electrolyte sheet according to claim 1 is dried and sealed.

[0091] S2'. In a water-free and oxygen-free glove box, place the positive electrode shell of the sodium ion battery with the opening facing upwards and lay it flat on a pad, place the positive electrode sheet in the center of the positive electrode shell, then drip the electrolyte to wet the surface of the electrode sheet, and place the electrolyte sheet of step S32 in the center of the electrode sheet; clamp the sodium metal sheet and place it in the center of the electrolyte sheet; finally, place the gasket and the spring in the center of the sodium metal sheet, cover the negative electrode shell and seal it to obtain a sodium ion battery.

[0092] Next, the preparation method of the sandwich structure NASICON composite electrolyte material and the preparation method of the nano-ion battery of the present application are described in detail with specific examples.

[0093] Preparation Example Preparation of sandwich structure NASICON composite electrolyte material

[0094] The NASICON composite electrolyte material is obtained by coating SbF3 and PVDF modification layers on both sides of the NASICON matrix electrolyte sheet, respectively. The sandwich structure NASICON composite electrolyte has good interface compatibility with the positive and negative electrodes, and the preparation method thereof is as follows:

[0095] S1. Preparation of NASICON matrix.

[0096] S11. Na2CO3, ZrO2, SiO2 and NH4H2PO4 were weighed in stoichiometric ratios and then dispersed in anhydrous ethanol and ball-milled for 12 h at a speed of 400 rpm. After ball-milling, the solution was poured into a watch glass and transferred to an oven at 80°C for 12 h to remove the ethanol. The dried powder was then sintered at 1000°C for 12 h.

[0097] S12. Grinding, ball milling and drying the powder obtained after sintering in sequence, wherein the ball milling and drying conditions are the same as above.

[0098] S13. The dried powder was pressed into a disc with a diameter of 15 mm and then placed in a crucible. The disc was sintered at 1200° C. for 10 h to obtain a NZSP electrolyte sheet.

[0099] S14. Finally, the NZSP electrolyte sheet is polished by a grinder and polisher (sandpaper mesh: 240, 400, 2000, 4000, 5000 mesh).

[0100] S2. Preparation of SbF3 and PVDF modified layer.

[0101] S21.SbF3 precursor solution preparation:

[0102] 0.1 g of SbF3 powder was dissolved in 10 mL of ethylene glycol dimethyl ether (DME) and stirred at room temperature for 12 h to obtain a SbF3 precursor solution.

[0103] S22. Preparation of PVDF precursor solution: Dissolve 0.25 g PVDF and 0.1 g NaTFSI in 7 mL N,N-dimethylformamide (DMF), and stir at 60° C. for 12 h to obtain a PVDF precursor solution.

[0104] S3. Preparation of sandwich structure PVDF-NASICON-SbF3 composite electrolyte.

[0105] S31. 50 μL of SbF3 precursor solution was added dropwise to one side of the NZSP electrolyte sheet, and the sheet was placed on a constant temperature heating table at 60°C and heated for 3 h to obtain SbF3-NZSP electrolyte.

[0106] S32. Add 60 μL of PVDF precursor solution to the other side of the electrolyte sheet, place it on a constant temperature heating table at 60°C and heat it for 3 hours to obtain PVDF-NZSP-SbF3 electrolyte.

[0107] S33. Add the SbF3 precursor solution dropwise to the other side of the NASICON electrolyte sheet, place it on a constant temperature heating table at 60°C and heat it for 3 hours to obtain SbF3-NASICON-SbF3 electrolyte.

[0108] Performance Characterization

[0109] The surface and cross section of the sandwich structure NASICON composite electrolyte sheet obtained in the preparation example were observed by scanning electron microscopy (SEM) and transmission electron microscopy (TEM). Figure 2 and Figure 3 shown.

[0110] in, Figure 2 This shows that the SbF3 layer and the PVDF layer are successfully attached to the surface of the NZSP electrolyte. The SbF3 particles and the Sb and F elements are evenly distributed on the surface of the NZSP electrolyte. Similarly, the PVDF coating is also evenly covered on the surface of the NZSP electrolyte, and the C and F elements are evenly distributed. This shows that SbF3 and PVDF do not aggregate on the surface of the NZSP electrolyte, indicating that the method is feasible.

[0111] Figure 3This shows that not only can the existence of the coating be proved, but also its thickness can be characterized. On the SbF3-NZSP, it can be clearly observed that there is a uniform coating on the surface. Moreover, the Sb and F elements are evenly distributed on the surface, and some appear inside the electrolyte. This shows that the SbF3 precursor solution can not only fill the scratches and pores on the surface of the NZSP, but also immerse in the crystal grains of the electrolyte, thus forming a continuous interface layer from the outside to the inside, which is more conducive to improving the stability of the interface with sodium metal. On the PVDF-NZSP, it can also be clearly observed that a smooth and flat PVDF layer of a certain thickness is laid flat on the surface of the NZSP electrolyte. Thanks to the synergistic effect of the two, the prepared sandwich structure NASICON composite electrolyte exhibits high specific capacity, excellent capacity retention and cycle stability in sodium ion batteries.

[0112] The present invention introduces a PVDF polymer layer on the side of the NASICON electrolyte in contact with the positive electrode. Figure 3 From the cross-sectional SEM image of PVDF-NZSP, we can see that there is a 2μm thick PVDF coating on the surface of the NASICON electrolyte sheet. Since PVDF polymer has a certain ductility, it can alleviate the problems of poor solid-solid interface contact and deterioration of interface contact caused by the volume expansion of the positive electrode active material during charging and discharging.

[0113] The sandwich structure NASICON composite electrolyte sheet material was observed by X-ray diffraction (XRD) and atomic force microscopy (AFM). Figure 4 and Figure 5 shown.

[0114] Figure 4 (a) illustrates the presence of SbF3 coating on the electrolyte surface, but the intensity is weak, which may be attributed to the thin thickness of the SbF3 coating, resulting in a weak signal. Figure 4 (b) illustrates that the drum peak located near 20.3° corresponds to the crystallization peak of PVDF, proving the successful introduction of PVDF coating on the electrolyte surface.

[0115] Figure 5 (a) It shows that even after grinding and polishing, there are still a lot of scratches on the surface of the NZSP electrolyte sheet, which will lead to uneven deposition of sodium ions and thus cause the growth of sodium dendrites. Ultimately, when used, the resulting solid-state metal battery will have poor cycle performance or poor electrochemical performance, resulting in reduced battery safety. Figure 5 (b) It shows that the scratches on the surface of the SbF3-NZSP electrolyte sheet are evenly covered by the SbF3 coating, and the surface roughness is significantly improved, which is more conducive to improving the wettability of the electrolyte sheet to molten sodium, thereby inhibiting the growth of sodium dendrites and providing the safety of sodium-ion batteries.

[0116] Preparation before application

[0117] The PVDF-NZSP-SbF3 composite electrolyte material obtained by drying was sealed under Ar atmosphere.

[0118] Application Example 1 Preparation of Sodium Ion Batteries

[0119] Preparation of sodium symmetric battery: A test battery is constructed using a CR 2032 button cell with sodium metal as the counter electrode / reference electrode. The test battery is operated in an argon-filled glove box. The positive electrode shell of the sodium ion battery is placed with the opening facing upward on a pad, and a sodium metal sheet is placed in the center of the positive electrode shell; then a SbF3-NZSP-SbF3 composite electrolyte sheet is clamped and placed in the center, and then a sodium metal sheet is clamped and placed in the center of the electrolyte sheet; finally, a gasket and a spring are placed in the center of the sodium metal sheet, and the negative electrode shell is covered and sealed to obtain a sodium symmetric sodium ion battery.

[0120] Preparation of the full battery: A CR 2032 button cell with sodium metal as the counter electrode / reference electrode is used to construct a test cell. The test cell is operated in an argon-filled glove box. The positive electrode shell of the sodium ion battery is opened upward and placed flat on a pad, and the Na3V2(PO4)3 positive electrode sheet is placed in the center of the positive electrode shell; then 1-2 drops of electrolyte [1M NaClO4 inEC / EMC (1:1) + 5% FEC] are added with a rubber-tipped dropper to wet the surface of the electrode sheet; then a PVDF-NZSP-SbF3 composite electrolyte sheet (the side coated with PVDF faces down) is clamped and placed in the center of the electrode sheet, and then a sodium metal sheet is clamped and placed in the center of the electrolyte sheet; finally, a gasket and a spring are placed in the center of the sodium metal sheet, and the negative electrode shell is covered and sealed to obtain a full-cell sodium ion battery.

[0121] Test Example 1 Electrochemical Performance Test of Sodium Symmetric Battery

[0122] The electrochemical performance (AC impedance spectrum and critical current density) of the sodium symmetric sodium ion battery prepared in Example 3 was tested using an electrochemical workstation. During the AC impedance spectrum test, the frequency test range was 1M to 0.1 Hz;

[0123] Depend on Figure 6 and Figure 7 It can be seen that in terms of interface impedance, the Na / NZSP / Na interface impedance is huge, about 1004Ωcm 2 In contrast, the interfacial impedance of the Na / SbF3-NZSP-SbF3 / Na sandwich structure symmetric cell is significantly reduced to 6Ωcm 2 This indicates that the NZSP electrolyte treated with the SbF3 modification layer has excellent sodium affinity. For the critical current density test, the Na / SbF3-NZSP-SbF3 / Na symmetric battery can withstand a maximum of 1.9 mA cm -2The current density of the Na / NZSP / Na symmetric cell is 0.2 mA cm -2 A short circuit occurs. It can be seen that the performance of the prepared sandwich structure NASICON composite electrolyte material is far superior to that of pure NASICON electrolyte material, and it has important uses in sodium ion batteries.

[0124] Through the in-situ conversion reaction between SbF3 and sodium metal, a Na x The ion-electron composite conductive layer composed of Sb alloy and NaF effectively improves the diffusion and conduction of ions at the interface, promotes the uniform deposition of sodium, and can significantly promote ion migration and improve interface stability.

[0125] Test Example 2 Electrochemical Performance Test of Full Battery

[0126] The electrochemical performance (cycle performance and rate performance) of the full battery prepared in Example 3 was tested using a multi-channel battery tester (Wuhan Blue Electric). In the cycle performance test, the current density was 0.2C and 2C; in the rate performance test, the current density was 0.1C and increased to 0.2C, 0.5C, 1C, 2C, and then returned to 0.1C;

[0127] Depend on Figure 8 and Fig. 9 It can be seen that in terms of cycle performance, at a current density of 0.2C, the capacity retention rate is as high as 92.17% after 720 cycles, and the average Coulomb efficiency is close to 100%, which is much better than the cycle performance of pure NASICON electrolyte at the same current density. At a high current density of 2C, the capacity retention rate is still as high as 92.91% after 450 cycles, and the average Coulomb efficiency is close to 99.9%. Fig.10 As can be seen, in terms of rate performance, the battery can work normally even at a current density of 2C and obtain 90.2mAh g -1 Specific capacity. It can be seen that the performance of the prepared sandwich structure NASICON composite electrolyte material is far superior to that of pure NASICON electrolyte material, which can significantly promote ion migration and improve interface stability, greatly improving the rate performance and cycle stability of sodium ion batteries, and therefore has important uses in sodium ion batteries.

[0128] This application cleverly uses NASICON electrolyte as a matrix, and coats SbF3 and PVDF on both sides of the NASICON electrolyte sheet by a simple solution drop coating method. After drop coating, a modified layer uniformly distributed on the surface of the electrolyte sheet is synthesized by drying under relatively mild conditions (60°C, Ar). At the same time, the PVDF-NZSP-SbF3 material is used as a sodium ion battery electrolyte, and excellent electrochemical performance (excellent cycle performance and rate performance) is obtained.

[0129] In terms of cycle performance, at a current density of 0.2C, the capacity retention rate can still be as high as 92.17% after 720 cycles. At a high current density of 2C, it can cycle more than 450 times and maintain a high reversible specific capacity and capacity retention rate. In terms of rate performance, even at a current density of 2C, the battery can work normally and obtain 90.2mAh g -1 The reversible specific capacity and sodium storage capacity of PVDF-NZSP-SbF3 are significantly better than those of NASICON electrolyte matrix, and thus it has important applications in sodium ion batteries.

[0130] Compared with the prior art, the beneficial effects of this application are:

[0131] The present application discloses a method for preparing a sandwich structure NASICON composite electrolyte material. A NASICON matrix is ​​obtained by a simple high-temperature solid-phase synthesis method, and a sandwich structure NASICON composite electrolyte is obtained by drying using a simple solution drop coating method.

[0132] First, through the in-situ conversion reaction between SbF3 and sodium metal, a Na x The ion-electron composite conductive layer composed of Sb alloy and NaF effectively improves the diffusion and conduction of ions at the interface, promotes the uniform deposition of sodium, and can significantly promote ion migration and improve interface stability, significantly improving the rate performance and cycle stability of sodium ion batteries.

[0133] Secondly, a PVDF polymer layer was introduced on the side of the NASICON electrolyte in contact with the positive electrode to alleviate the problems of poor solid-solid interface contact and deterioration of interface contact caused by the volume expansion of the positive electrode active material during charging and discharging.

[0134] In the third aspect, the PVDF-NZSP-SbF3 composite electrolyte material is applied to the preparation of a button battery, which is made of an electrode sheet, a sodium metal sheet, an electrolyte sheet, a spring, a gasket, and a positive and negative electrode shell. The button battery prepared by the NASICON composite electrolyte material used in this application has excellent electrochemical properties.

[0135] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials, or characteristics described in conjunction with the embodiments or examples are included in at least one embodiment or example of the present application. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials, or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.

[0136] Although several embodiments of the present application have been shown and described, those skilled in the art will appreciate that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present application, and that the scope of the present application is defined by the claims and their equivalents.

Claims

1. A sandwich structure NASICON composite electrolyte material, characterized in that: The sandwich structure NASICON composite electrolyte material uses NASICON type oxide ceramic as a matrix, and introduces a polymer layer PVDF and an inorganic layer AB3 on both sides of the NASICON type oxide ceramic sheet, respectively, wherein A is one or more of Bi, Sb and Sn, and B is one or more of I, Br and F.

2. The method for preparing the sandwich structure NASICON composite electrolyte material according to claim 1 comprises the following steps: S1. Na2CO3, ZrO2, SiO2 and NH4H2PO4 were weighed in a stoichiometric ratio, dispersed in anhydrous ethanol, ball-milled, pressed and sintered, and finally polished to obtain a pure NASICON electrolyte sheet; S2. The SbF3 powder was dissolved in ethylene glycol dimethyl ether and stirred to obtain a SbF3 precursor solution, and PVDF and NaTFSI were dissolved in N,N-dimethylformamide and stirred to obtain a PVDF precursor solution; S3. The SbF3 precursor solution is added dropwise to one side of the NASICON electrolyte sheet to obtain the SbF3-NZSP electrolyte, and the PVDF precursor solution is added dropwise to the other side of the SbF3-NZSP electrolyte to obtain the PVDF-NZSP-SbF3 electrolyte.

3. The method for preparing the sandwich structure NASICON composite electrolyte material according to claim 2, characterized in that: In step S1, the Na2CO3 and NH4H2PO4 should be in appropriate excess, and the excess of Na2CO3 and NH4H2PO4 is about 10-15%.

4. The method for preparing the sandwich structure NASICON composite electrolyte material according to claim 2, characterized in that: The entire experimental operation of step S2 was carried out in a glove box under an Ar gas atmosphere with H2O<0.1, O2<0.

1.

5. The method for preparing the sandwich structure NASICON composite electrolyte material according to claim 3, characterized in that: In step S1, the ball milling time is 12 hours, the sintering temperature is 1000° C., and the time is 12 hours.

6. The method for preparing the sandwich structure NASICON composite electrolyte material according to claim 4, characterized in that: In step S2, the stirring time is 12 hours.

7. The method for preparing the sandwich structure NASICON composite electrolyte material according to claim 2, characterized in that: In step S3, the amount of the SbF3 precursor solution added is 50 μL, and the amount of the PVDF precursor solution added is 60 μL.

8. The method for preparing the sandwich structure NASICON composite electrolyte material according to claim 7, characterized in that: In step S3, the inert gas is an argon atmosphere.

9. A sodium ion battery, characterized in that: The electrolyte in the sodium ion battery is the sandwich structure NASICON composite electrolyte material according to claim 1.

10. The method for preparing a sodium ion battery according to claim 9, characterized in that: The following steps are involved: S1 '. The sandwich structure NASICON composite electrolyte sheet according to claim 1 is dried and sealed. S2'. In a water-free and oxygen-free glove box, place the positive electrode shell of the sodium ion battery with the opening facing upwards and lay it flat on a pad, place the positive electrode sheet in the center of the positive electrode shell, then drip the electrolyte to wet the surface of the electrode sheet, and place the electrolyte sheet of step S3 in the center of the electrode sheet; clamp the sodium metal sheet and place it in the center of the electrolyte sheet; finally, place the gasket and the spring sheet in the center of the sodium metal sheet, cover the negative electrode shell and seal it to obtain a sodium ion battery.

Citation Information

Patent Citations

  • Solid electrolyte interface modification method and all-solid-state sodium battery

    CN115911525A

  • Solid electrolyte with functional middle layer with gradient structure and preparation method and application of solid electrolyte

    CN116960446A

  • Asymmetric composite electrolyte and preparation method and application thereof

    CN117936889A

  • Quick-charge type solid electrolyte, all-solid-state battery and preparation method of positive electrode material

    CN118248938A

Cited By

  • Composite solid electrolyte, solid sodium metal battery and preparation method of composite solid electrolyte and solid sodium metal battery

    CN120015909A

  • A composite solid-state electrolyte and a solid-state sodium metal battery and a preparation method thereof

    CN120015909B