Flame retardant sheet
By maintaining the aggregation of functional particles through a combination of inorganic fibers and microfibers, combined with an appropriate amount of binder, the problem of the trade-off between texture and yield of flame-retardant sheet materials is solved, and efficient functional particle loading and flame-retardant properties are achieved.
Patent Information
- Application Number
- CN202180045472.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-07-05
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-07-05
AI Technical Summary
While improving the efficiency of fiber-loaded functional particles, the existing technology is difficult to maintain the excellent texture and yield of the flame-retardant sheet at the same time. Excessive aggregation of the agent will cause the texture to deteriorate and the yield to decrease.
Adopting a combination of inorganic fibers, functional particles and microfibers, maintaining the aggregation of functional particles and microfibers through inorganic fibers, using binder components to improve loading efficiency and texture, while controlling the size distribution of particles and fibers to optimize flame retardancy sex.
A flame-retardant sheet with excellent texture and yield is achieved, ensuring efficient functional particle loading and flame-retardant performance.
Smart Images

Figure CN115768944B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a flame retardant sheet. Background Art
[0002] Conventionally, when obtaining a sheet material in which functional particles are supported on fibers, the supporting efficiency of the functional particles is improved by including fibrillated organic fibers.
[0003] However, in order to further impart flame retardancy to the sheet itself, it is necessary to reduce the content of organic fibers.
[0004] In the past, for example, the content described in Patent Document 1 has been proposed regarding flame-retardant sheets. Patent Document 1 describes a flame-retardant and heat-resistant paper, characterized in that it is made by mixing 5 to 100 parts by weight of fiber material and / or other additives with 100 parts by weight of a mixture of 90 to 20% by weight of calcium silicate and 10 to 80% by weight of magnesium oxysulfate. Moreover, it is described that this flame-retardant and heat-resistant paper has the greatest feature of mixing magnesium oxysulfate with calcium silicate, which has flame retardancy and reinforcing effects, and the calcium silicate and magnesium oxysulfate act synergistically, have good papermaking properties and ensure a high yield, improve flame retardancy, and exert a very significant effect of excellent heat-resistant shape retention.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Laid-Open No. 5-230790 Summary of the invention
[0008] Problem that the invention aims to solve
[0009] As mentioned above, when it is desired to further impart flame retardancy to a sheet material loaded with functional particles on a fiber, the loading efficiency of the functional particles can be improved by adding an aggregating agent. However, if an aggregating agent is added, there is a tendency that the texture of the sheet material deteriorates due to over-aggregation. That is, the inventors have found that the texture and yield are in a compromise relationship. If it is desired to obtain a flame retardant sheet material with excellent texture, the yield decreases, and on the contrary, if it is desired to increase the yield, the texture tends to deteriorate.
[0010] The present invention aims to solve the above-mentioned problems. That is, the present invention aims to provide a flame-retardant sheet having excellent texture and yield.
[0011] Solutions for solving problems
[0012] The present inventors have conducted intensive studies to solve the above-mentioned problems and have completed the present invention.
[0013] The present invention includes the following (1) to (9).
[0014] (1) A flame-retardant sheet comprising: inorganic fibers, functional particles, a binder component and fine fibers,
[0015] At least a portion of the functional particles have a particle size of 2.5 μm or less,
[0016] The fine fibers and the functional particles are aggregated and held by the inorganic fibers.
[0017] (2) The flame-retardant sheet according to (1) above, wherein
[0018] The fiber diameter of the inorganic fibers exceeds 2 μm,
[0019] The fiber diameter of the fine fibers is 2 μm or less.
[0020] (3) The flame-retardant sheet according to (1) or (2) above, wherein the fine fibers are made of an inorganic substance.
[0021] (4) The flame-retardant sheet according to any one of (1) to (3) above, wherein the fine fibers are mineral fibers and / or fibrous growth crystals.
[0022] (5) The flame-retardant sheet according to any one of (1) to (4) above, which contains no fibril fibers.
[0023] (6) The flame-retardant sheet according to any one of (1) to (5) above, wherein the organic component is 11 wt % or less.
[0024] (7) The flame-retardant sheet according to any one of (1) to (6) above, comprising two or more types of the functional particles.
[0025] (8) The flame-retardant sheet according to any one of (1) to (7) above, wherein the functional particles have a number average particle size of 1 to 20 μm.
[0026] (9) The flame-retardant sheet according to any one of (1) to (8) above, characterized in that the ratio of the number average particle size of the functional particles to the average fiber diameter of the fine fibers (number average particle size of the functional particles / average fiber diameter of the fine fibers) is 1 to 100.
[0027] Effects of the Invention
[0028] According to the present invention, a flame-retardant sheet having excellent texture and yield can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is a magnified photograph (SEM image) obtained by magnifying the surface of the flame-retardant sheet obtained in the example to 10,000 times using a scanning electron microscope (SEM).
[0030] Figure 2 This is a magnified photograph (SEM image) obtained by magnifying the surface of the flame-retardant sheet obtained in another example by 1000 times using a scanning electron microscope (SEM). DETAILED DESCRIPTION
[0031] <Flame-retardant sheet of the present invention>
[0032] The flame-retardant sheet of the present invention will be described.
[0033] The flame-retardant sheet of the present invention is a flame-retardant sheet characterized by comprising: inorganic fibers, functional particles, a binder component and fine fibers, at least a portion of the functional particles having a particle size of 2.5 μm or less, and the fine fibers and the functional particles are aggregated and held by the inorganic fibers. This flame-retardant sheet is hereinafter also referred to as "the flame-retardant sheet of the present invention".
[0034] <Inorganic Fiber>
[0035] The inorganic fibers contained in the flame-retardant sheet of the present invention will be described.
[0036] In the flame retardant sheet of the present invention, the inorganic fiber functions as a base material. Therefore, the inorganic fiber plays a role in maintaining the shape of the flame retardant sheet of the present invention. In addition, the inorganic fiber sometimes also plays a role in assisting the metal mesh to peel off, assisting the tensile strength, and suppressing the surface shrinkage during strong heat. Furthermore, when it becomes above the melting temperature, it sometimes also functions as an inorganic binder.
[0037] Inorganic fiber is a fibrous inorganic substance.
[0038] Examples of the inorganic fibers include glass fibers, asbestos, refractory ceramic fibers, AES fibers, silica fibers, alumina fibers, and glass fibers.
[0039] The inorganic fibers are preferably glass fibers, silica fibers, and alumina fibers because it is easy to ensure a fiber length that can increase the yield in production.
[0040] The fiber diameter of the inorganic fibers is preferably greater than 2 μm.
[0041] In the flame-retardant sheet of the present invention, it is preferred that the fibers formed of an inorganic substance having a fiber diameter exceeding 2 μm are inorganic fibers.
[0042] The fiber diameter of the inorganic fibers is more preferably 3 μm or more and 20 μm or less, and further preferably 5 μm or more and 10 μm or less.
[0043] The fiber diameter of inorganic fibers can be an area diameter (equivalent diameter of a circle of equal area) derived by calculating the cross-sectional area of the inorganic fibers based on a vertical cross-section of the inorganic fibers photographed under a microscope (for example, using known software) and calculating the diameter of a circle having the same area as the aforementioned cross-sectional area.
[0044] The average fiber diameter of the inorganic fibers is more preferably 3 μm or more and 20 μm or less, and further preferably 5 μm or more and 10 μm or less.
[0045] Here, the average fiber diameter of the inorganic fibers refers to a diameter measured by the following method.
[0046] The cross-sectional area of the inorganic fiber can be calculated based on a vertical cross-section of the inorganic fiber photographed by a microscope (for example, using known software), and the average value of the area diameter (for example, the average value of 20 fibers) can be derived by calculating the diameter of a circle having the same area as the aforementioned cross-sectional area.
[0047] The fiber length of the inorganic fibers is not particularly limited, but the average fiber length of the inorganic fibers is preferably 0.5 to 10 mm, more preferably 1.5 to 6 mm.
[0048] Here, the length of the inorganic fibers (fiber length) refers to the length measured by the following method.
[0049] The length of 100 inorganic fibers randomly selected from a SEM image of the surface of the flame-retardant sheet of the present invention magnified 100 times using a scanning electron microscope (SEM) was measured, and the lengths were simply averaged to obtain the length.
[0050] In order for the inorganic fibers to function as a base material, it is desirable that the inorganic fibers have an aspect ratio (ratio of fiber length÷fiber diameter) of 50 or more.
[0051] In order to impart strength to the flame-retardant sheet, the average fiber diameter is preferably 2 to 20 μm, more preferably 3 to 20 μm, and further preferably 5 to 13 μm.
[0052] The content of the inorganic fibers contained in the flame-retardant sheet of the present invention is not particularly limited.
[0053] The content of the inorganic fibers in the flame-retardant sheet of the present invention is preferably 4 to 75% by mass, more preferably 6 to 60% by mass, and even more preferably 8 to 50% by mass.
[0054] Here, the content of the inorganic fibers contained in the flame-retardant sheet of the present invention refers to a value measured by the following method.
[0055] In the SEM image obtained by magnifying the surface of the flame-retardant sheet of the present invention to 10,000 times using a scanning electron microscope (SEM), the area of all components occupied within its field of view is calculated using an image processing device, and the volume ratio is converted by setting it to the cube and then multiplied by the specific gravity to obtain the mass ratio and calculate the content of inorganic fibers.
[0056] <Functional particles>
[0057] The functional particles contained in the flame-retardant sheet of the present invention will be described.
[0058] In the flame-retardant sheet of the present invention, the functional particles and the fine fibers described below are aggregated and held by the inorganic fibers.
[0059] In the flame-retardant sheet of the present invention, the functional particles are not particularly limited as long as they are particles having a function for achieving a certain purpose, such as particles that show heat absorption through thermal decomposition and structural phase change, particles that show thermal insulation due to a porous structure and fine particle size, particles that have the ability to adsorb moisture and gas, etc.
[0060] Examples of the functional particles include aluminum hydroxide, titanium oxide, silica gel, zeolite, ash balls, activated carbon, and molecular sieves.
[0061] The flame-retardant sheet of the present invention preferably contains two or more types of functional particles.
[0062] In addition to containing more than two kinds of functional particles with different compositions, containing more than two kinds of functional particles also means containing more than two kinds of functional particles of the same type but different sizes. For example, when the particle size distribution of the functional particles has more than two peaks, the flame retardant sheet of the present invention contains more than two kinds of functional particles. That is, it is not limited to containing more than two kinds of different kinds of functional particles, and it can also contain more than two kinds of functional particles of the same type but different particle sizes.
[0063] The particle size of the functional particles is not particularly limited. The number average particle size of the functional particles is preferably 0.1 to 50 μm, more preferably 0.5 to 35 μm, and even more preferably 1 to 20 μm.
[0064] The number average particle size of the functional particles herein refers to a value obtained by the following measurement. For example, the functional particles are recovered from the flame retardant sheet, and the particles dispersed in the liquid are directly photographed, and the number average particle size can be obtained by using a flow-based image analysis device (e.g., FPIA-3000 manufactured by Sysmex) that can analyze / analyze based on image processing of the photographed data.
[0065] In addition, at least a portion of the functional particles have a particle size of 2.5 μm or less. That is, the functional particles have a particle size distribution with a certain degree of width, but contain particles of 2.5 μm or less. The particle size of all functional particles contained in the flame-retardant sheet of the present invention can be 2.5 μm or less. In addition, the functional particles with a particle size of 2.5 μm or less preferably contain 0.5 to 99% by mass, more preferably 2 to 98% by mass, relative to the total amount of the functional particles.
[0066] The ratio of functional particles having a size of 2.5 μm or less contained in the functional particles refers to a value measured as follows.
[0067] For example, functional particles are recovered from flame-retardant sheets, and particles dispersed in liquid are directly photographed, which can be obtained by using a flow-based image analysis device (e.g., FPIA-3000 manufactured by Sysmex) that can analyze / analyze based on image processing of the photographed data. From the data of each functional particle measured, the cumulative value of the frequency of occurrence of particles corresponding to a range of 2.5 μm or less is calculated to determine the ratio of the measured object to the entire functional particle, thereby determining the ratio of functional particles below 2.5 μm.
[0068] The D50 particle size of the functional particles is not particularly limited, but is preferably 0.1 to 50 μm, more preferably 0.5 to 35 μm, and even more preferably 1 to 20 μm.
[0069] Here, the D50 particle size of the functional particles refers to a value measured as follows.
[0070] For example, functional particles are recovered from flame-retardant sheets, and particles dispersed in liquid are directly photographed, which can be obtained by using a flow-based image analysis device (e.g., FPIA-3000 manufactured by Sysmex) that can analyze / analyze based on image processing of the photographed data. The data of each functional particle measured can be obtained based on the particle diameter at the cumulative value of 50% in the particle size distribution based on the number of particles.
[0071] The content of the functional particles contained in the flame-retardant sheet of the present invention is not particularly limited.
[0072] The content of the functional particles in the flame-retardant sheet of the present invention is preferably 20 to 95% by mass, more preferably 30 to 90% by mass, and further preferably 40 to 80% by mass.
[0073] Here, the content of functional particles contained in the flame-retardant sheet of the present invention refers to a value measured by the following method. In a SEM image obtained by magnifying the surface of the flame-retardant sheet of the present invention to 10,000 times using a scanning electron microscope (SEM), the area of all components occupied in the field of view is obtained using an image processing device, and the area is converted to a volume ratio by setting it to the third power, and then multiplied by the specific gravity to obtain a mass ratio, and the content of the functional particles is calculated.
[0074] <Binder ingredients>
[0075] The binder component contained in the flame-retardant sheet of the present invention will be described.
[0076] The binder component in the flame-retardant sheet of the present invention is not particularly limited as long as it can be bonded to other components of the flame-retardant sheet by dissolving or melting, or can be chemically or physically bonded or aggregated with other components of the flame-retardant sheet.
[0077] As a binder component, there is no limitation as long as it plays the role of connecting other components of the flame retardant sheet. For example, pulp, aggregating agent, reinforcing agent can be cited, and further organic components such as acrylic resin, polyester resin, polyethylene terephthalate resin (PET resin), polyolefin resin, vinyl acetate resin, styrene resin, polyurethane resin, phenolic resin can be cited. Pulp has the effect of assisting the peeling of the self-coated metal wire mesh, assisting the aggregation of other components, and enhancing the tensile strength (hydrogen bond) of the flame retardant sheet, so it is preferred. Aggregating agent is preferred from the aspect of easily retaining functional particles in the flame retardant sheet in advance. As aggregating agent, specifically, known aggregating agents such as aluminum sulfate, polyacrylamide, epoxy resin can be cited. Acrylic resin is preferred because it is easy to enhance the tensile strength of the flame retardant sheet, assist the aggregation of other components, and inhibit the falling of functional particles. PET fiber is preferred because it is easy to assist the peeling of the self-coated metal wire mesh and enhance the tensile strength.
[0078] The shape of the binder component is not limited. For example, it can be granular (including powder, dispersion, emulsion), liquid, fibrous. By using a variety of binder components such as the strength improvement of the flame retardant sheet, the imparting of flexibility, and the prevention of the functional particles from falling off the sheet (improving the yield), these functions can also exist simultaneously.
[0079] Here, the fiber diameter of the fibrous binder component means a diameter measured by the same method as the fiber diameter of the inorganic fiber.
[0080] The content of the binder component contained in the flame-retardant sheet of the present invention is not particularly limited.
[0081] The content of the binder component in the flame-retardant sheet of the present invention is preferably 0.5% by mass or more, more preferably 1% by mass or more, and even more preferably 2% by mass or more.
[0082] The content of the binder component in the flame-retardant sheet of the present invention is preferably 25% by mass or less, more preferably 16% by mass or less, and even more preferably 2% by mass or less.
[0083] It should be noted that the content of the binder component in the flame-retardant sheet of the present invention is determined as follows. First, the flame-retardant sheet of the present invention is dried at 120°C until it becomes constant weight, heated at 525°C for 1 hour, and then cooled to room temperature in a dryer. Then, the mass difference (X) before and after heating at 525°C is calculated.
[0084] Next, the flame-retardant sheet of the present invention is subjected to fluorescent X-ray analysis to perform qualitative / quantitative analysis of the inorganic substances contained therein. Then, the weight loss (Y) derived from the inorganic substances when heated at 525°C (mainly from crystal water) is determined. The weight loss (Y) can be calculated based on a known value, or an inorganic substance of the same composition can be obtained and heated at 525°C to measure the weight loss, thereby determining the weight loss (Y).
[0085] Then, the amount of organic functional particles obtained by the above method, the amount of organic fine fibers obtained by the method described below, and the weight loss (Y) of inorganic origin are subtracted from the mass difference (X), and the remainder is taken as the amount of organic binder component. Next, in the SEM image obtained by magnifying the surface of the flame-retardant sheet of the present invention to 10,000 times using a scanning electron microscope (SEM), the area of each of all components in its field of view is obtained using an image processing device, and the volume ratio is converted by setting it to the third power, and then multiplied by the specific gravity to obtain the mass ratio and calculate the content of the inorganic binder component. Next, the obtained amounts of organic and inorganic binder components are added together to obtain the content of the binder component in the flame-retardant sheet of the present invention.
[0086] <Microfiber>
[0087] The fine fibers contained in the flame-retardant sheet of the present invention will be described.
[0088] In the flame-retardant sheet of the present invention, the fine fibers and the functional particles are aggregated and held by the inorganic fibers.
[0089] Examples of fine fibers include natural mineral fibers such as sepiolite, wollastonite, and attapulgite, mineral fibers such as artificial mineral fibers such as microglass fibers, fibrous growth crystals (whiskers) such as potassium titanate fibers, calcium carbonate fibers, and calcium silicate fibers, microfiber cellulose, and organic fibers such as fibrillated aramid.
[0090] The fine fibers are preferably formed of inorganic substances. Among mineral fibers, sepiolite is preferred. Since sepiolite exhibits dry consolidation properties such that when a slurry dispersed in water is dried, it will agglomerate in this form, and therefore, it is easy to play the role of retaining the functional particles in the flame-retardant sheet in advance. In addition, since the crystal water is dehydrated by heating, it is easy to contribute to flame retardancy. Among fibrous growth crystals (whiskers), potassium titanate fibers are preferred. Potassium titanate fibers may include fibers with a fiber length of 10 μm or less.
[0091] The fine fibers preferably have a fiber diameter of 2 μm or less.
[0092] In the flame-retardant sheet of the present invention, it is preferred that the fibers having a fiber diameter of 2 μm or less are fine fibers.
[0093] The fiber diameter of the fine fibers is preferably 0.05 μm or more, more preferably 0.1 μm or more, and the fiber diameter of the fine fibers is preferably 2.0 μm or less, more preferably 1.0 μm or less, and further preferably 0.5 μm or less.
[0094] The fiber diameter of a microfiber herein refers to a diameter measured by the following method: the cross-sectional area of the microfiber is calculated based on a vertical cross section of the microfiber photographed with a microscope (for example, using known software), and the area diameter is derived by calculating the diameter of a circle having the same area as the cross-sectional area.
[0095] The average fiber diameter of the fine fibers is more preferably 0.05 μm or more, and further preferably 0.1 μm or more.
[0096] The average fiber diameter of the fine fibers is preferably 2.0 μm or less, more preferably 1.0 μm or less, and further preferably 0.5 μm or less.
[0097] The average fiber diameter of the microfibers herein refers to a diameter measured by the following method, which can be an average value of area diameters derived by calculating the diameter of a circle having the same area as the cross-sectional area based on a vertical cross section of the microfibers photographed with a microscope (for example, using known software) (for example, an average value of 20 fibers).
[0098] The ratio of the number average particle size of the functional particles to the average fiber diameter of the fine fibers (number average particle size of the functional particles / average fiber diameter of the fine fibers) is preferably 1 to 100, more preferably 3 to 65. The reason is as follows Figure 2 The microfibers have the effect of aggregating the functional particles (particularly particles with a small particle size) in a manner that allows them to be more well intertwined.
[0099] The ratio of the D50 particle size of the functional particles to the average fiber diameter of the fine fibers (D50 particle size of the functional particles / average fiber diameter of the fine fibers) is preferably 1 to 180, more preferably 3 to 150. The reason is as follows Figure 2 The microfibers have the effect of aggregating the functional particles (particularly particles with a small particle size) in a manner that allows them to be more well intertwined.
[0100] The length of the fine fibers is not particularly limited, but the length of the fine fibers is preferably 1 to 3000 μm, more preferably 10 to 500 μm.
[0101] The aspect ratio of the fine fibers is preferably 5 to 6000. When the aspect ratio is 5 or more, the functional fine particles can be easily captured. When the aspect ratio is 6000 or less, the texture of the flame-retardant sheet can be easily improved.
[0102] In addition, the length of a microfine fiber means the length measured by the following method.
[0103] The method can be a method in which fine fibers dispersed in water are photographed in a flowing state and the fiber length is determined by image analysis from the photograph (such an image analysis type fiber length measuring instrument includes a fiber tester manufactured by L&W). Alternatively, the length of 100 randomly selected fine fibers can be measured in an SEM image obtained by magnifying the surface of the flame-retardant sheet of the present invention to 100 times using a scanning electron microscope (SEM) JSM-7001F manufactured by JEOL Ltd., and the length of these fibers can be determined by simply averaging them.
[0104] The content of the fine fibers contained in the flame-retardant sheet of the present invention is not particularly limited.
[0105] The content of the fine fibers in the flame-retardant sheet of the present invention is preferably 0.1 to 35% by mass, more preferably 0.5 to 20% by mass, and even more preferably 1 to 10% by mass.
[0106] Here, the content of fine fibers contained in the flame-retardant sheet of the present invention refers to a value measured by the following method.
[0107] In the SEM image obtained by magnifying the surface of the flame-retardant sheet of the present invention to 10,000 times using a scanning electron microscope (SEM), the area of all components occupied within its field of view is calculated using an image processing device, and the volume ratio is converted by setting it to the cube and then multiplied by the specific gravity to obtain the mass ratio and calculate the content of fine fibers.
[0108] The flame-retardant sheet of the present invention contains inorganic fibers, functional particles, a binder component, and fine fibers as described above, but may contain other components.
[0109] As other components, a water repellent, a coloring agent, etc. are mentioned, for example.
[0110] The flame-retardant sheet of the present invention preferably does not contain fibril fibers. By not containing fibril fibers, the surface property, which is one of the causes of combustion, is suppressed to a low level, and flame retardancy is easily improved.
[0111] Fibrillar fibers refer to fibers with a fibrous microstructure of several nanometers to several micrometers in size, which are composed of organic matter. Examples of fibrillary fibers include natural cellulose fibers, regenerated cellulose fibers, aramid fibers (Teijin: Towaron pulp, Dupont: Kevlar pulp, etc.), acrylic fibers (Toyobo: BiPUL, Sterling Fibers: CFF, etc.), polyacrylate fibers, and polyethylene synthetic pulp (Mitsui Chemicals: SWP, etc.).
[0112] The organic component contained in the flame-retardant sheet of the present invention is preferably 20 wt% or less, preferably 11 wt% or less, more preferably 6 wt% or less, and further preferably 5 wt% or less. When it is 11 wt% or less, flame retardancy can be easily obtained.
[0113] The content of the organic component contained in the flame-retardant sheet of the present invention refers to a value measured as follows.
[0114] The components other than the ash obtained by the ash content test method (525°C combustion method) of JIS P8251 paper, board and pulp are regarded as organic components. Here, when the weight loss caused by the release of crystal water of inorganic substances is generated by the ashing treatment at 525°C, the weight loss of inorganic substances after the ashing treatment is subtracted to obtain the content of organic components. It should be noted that for the weight loss caused by the release of crystal water of inorganic substances, the flame-retardant sheet of the present invention is first subjected to fluorescent X-ray analysis to perform qualitative / quantitative analysis on the inorganic substances contained. Then, the weight loss of inorganic substances when heated at 525°C is obtained. Here, the weight loss can be calculated based on the known value, or the inorganic substances of the same composition can be obtained and the weight loss can be measured by heating at 525°C to obtain the weight loss.
[0115] The size, thickness, etc. of the flame-retardant sheet of the present invention are not particularly limited.
[0116] The thickness of the flame-retardant sheet of the present invention is preferably 0.1 to 10 mm.
[0117] The thickness of the flame-retardant sheet of the present invention is a value obtained by measuring the thickness at any 50 points of the flame-retardant sheet of the present invention with a micrometer, and simply averaging the measured values to obtain the thickness of the flame-retardant sheet of the present invention.
[0118] The flame retardant sheet of the present invention preferably has a mass per unit area of 80 to 2000 g / m 2 , more preferably 80 to 1000 g / m 2 .
[0119] The density of the flame-retardant sheet of the present invention depends on the true density of the functional particles used, but is preferably 0.1 to 1 g / cm 3 .
[0120] In addition, the density of the flame-retardant sheet of the present invention refers to a value measured in accordance with JIS Z 8807:2012 "Determination method of density and specific gravity of solids".
[0121] The method for producing the flame-retardant sheet of the present invention is not particularly limited.
[0122] For example, it can be manufactured by a powder-loaded papermaking method. The powder-loaded papermaking method refers to a method of using a papermaking slurry in which powder is dispersed to make paper using a general papermaking process. More specifically, after the fiber and the powder are stirred with a dispersion medium (water, an organic solvent, etc.), a papermaking slurry is prepared, and a square manual papermaking device (for example, manufactured by Toyo Seiki Co., Ltd.) is used to make a sheet, and the sheet is dried with a drying device for dry sheets, thereby obtaining a flame-retardant sheet. The process of the powder-loaded papermaking method can be intermittent or continuous.
[0123] Example
[0124] <Examples 1 to 21 and Comparative Example 1>
[0125] Inorganic fibers, functional particles, binder components, fine fibers and aggregating agents of the types shown in Tables 2, 3 and 4 are mixed and dispersed in the contents shown in Tables 2, 3 and 4 to obtain a slurry, which is then used to prepare a flame-retardant sheet by a powder-loaded papermaking method.
[0126] In any of the Examples and Comparative Examples, the thickness of the obtained flame-retardant sheet was about 1 mm.
[0127] In addition, the details of each component are as follows.
[0128] <Inorganic Fiber>
[0129] As inorganic fibers, glass wool having an average fiber diameter of 5 μm, glass fibers having an average fiber diameter of 7 μm, and rockwool having an average fiber diameter of 8 μm were prepared and used.
[0130] <Functional particles>
[0131] As functional particles, a plurality of types of aluminum hydroxide, silica gel, heavy calcium carbonate, hydrotalcite, and HASClay were prepared and used. In addition, in Examples 5, 18, 20, and 21, two types of functional particles were used.
[0132] <Binder ingredients>
[0133] As the binder component, softwood pulp (fiber diameter: 20 to 40 μm), acrylic resin, and PET fiber (manufactured by Teijin Ltd., TA04PN, fiber diameter: 3 μm) were prepared and used. In Examples 4, 5, 18, and 19, two types of binder components were used.
[0134] <Microfiber>
[0135] As fine fibers, sepiolite, potassium titanate whiskers, and microfibril cellulose were prepared and used. Details of each are shown below.
[0136] ·Sepiolite: Milcon, Showa KDE Co., Ltd. (average fiber diameter: 0.1 μm or 0.3 μm)
[0137] Potassium titanate whiskers: (average fiber length: 15 μm, average fiber diameter: 0.3 μm)
[0138] · Microfibril cellulose: Serish KY100G, manufactured by Daicel Co., Ltd.
[0139] <Aggregating agent>
[0140] As one of the binder components, a coagulant (High Holder C-503 manufactured by Kurita Industry Co., Ltd.) was used.
[0141] Next, the yield of the flame-retardant sheets obtained in the examples and comparative examples was determined, the texture was evaluated, and a comprehensive evaluation was performed based on these. In addition, the handling strength, heat-resistant shape retention, and flammability were evaluated.
[0142] The yield, texture, handling strength, heat resistance and shape retention, and flammability were measured and evaluated as follows.
[0143] <Yield>
[0144] The yield was calculated according to the following calculation.
[0145] Yield (%) = actual weight of one flame-retardant sheet after drying (g) × 100 / actual weight of one sheet of raw materials (g)
[0146] In addition, the case where the yield was less than 70% was evaluated as ×, the case where it was 70% or more and less than 80% was evaluated as △, and the case where it was 80% or more was evaluated as ○.
[0147] <Texture>
[0148] The surface of the flame-retardant sheet was observed and the texture was classified as follows. The description in the table below is also shown.
[0149] ◎: There are no aggregates and no depth of the sheet.
[0150] ○: There is a slight difference in depth, but the uniformity is good.
[0151] △: Although there is some unevenness in depth, it is at a practical level.
[0152] ×: Agglomerates are present and unevenness in depth is also noticeable.
[0153] <Overall Evaluation>
[0154] Based on the results of yield and texture, comprehensive evaluation was performed using Table 1.
[0155] [Table 1]
[0156] Table 1
[0157]
[0158] <Combustibility>
[0159] The flame retardant sheet was cut into strips 13 mm wide and hung in a manner such that the length direction was vertical. Then, a flame adjusted to a height of 20 mm was irradiated from below for 10 seconds at a position 10 mm below the sheet. In this case, it was determined whether the burning portion was less than 5 cm from below.
[0160] The yield, texture, and comprehensive evaluation based on these are shown in Table 2, Table 3, and Table 4. It should be noted that the flame-retardant sheets obtained in all Examples were good in handling strength, heat-resistant shape retention, and flammability.
[0161] [Table 2]
[0162]
[0163] [Table 3]
[0164]
[0165] [Table 4]
[0166]
[0167] Furthermore, the surface of the flame-retardant sheet obtained in Example 5 was observed by magnifying it 10,000 times using SEM. The obtained SEM image is shown in Figure 1 . Figure 1 (a) is a SEM image (enlarged photograph) of the surface of the flame-retardant sheet. Figure 1 (b) is a SEM image (enlarged photo) of the inner surface. Figure 1 It can be confirmed that the sepiolite as fine fibers aggregates and holds the aluminum hydroxide as functional particles while being held by the inorganic fibers (glass fibers).
[0168] In addition, the surface of the flame-retardant sheet obtained in Example 14 was observed by magnifying it 1000 times using SEM. The obtained SEM image is shown in FIG. Figure 2 .according to Figure 2 It was confirmed that potassium titanate whiskers as fine fibers aggregated and held silica gel as functional particles while being held by inorganic fibers (glass fibers).
[0169] This application claims the benefit of priority based on Japanese patent application No. 2020-118869, filed on Jul. 10, 2020, the disclosure of which is incorporated herein by reference in its entirety.
[0170] Industrial Applicability
[0171] The flame-retardant sheet of the present invention can be used as, for example, a fire-resistant material, a heat insulating material that functions under high temperature conditions, and the like.
Claims
1. A flame retardant sheet, characterized in that: Contains: inorganic fibers, functional particles, binder components and microfibers, The content of the inorganic fibers is 10 to 75% by mass. The particle size of at least a portion of the functional particles is 2.5 μm or less, As the binder component, at least one selected from the group consisting of pulp, acrylic resin, polyester resin, polyethylene terephthalate resin (PET resin), polyolefin resin, vinyl acetate resin, styrene resin, polyurethane resin and phenolic resin is used, The fiber diameter of the microfiber is 0.05 to 2 μm, and the length of the microfiber is 1 to 3000 μm. The fine fibers are at least one selected from the group consisting of sepiolite, wollastonite, attapulgite, microglass fibers, potassium titanate fibers, calcium carbonate fibers, calcium silicate fibers, microfiber cellulose, and fibrillated aramid. The fine fibers are aggregated with the functional particles and held by the inorganic fibers. The content of the fine fibers is 0.1 to 35% by mass. The ratio of the number average particle diameter of the functional particles to the average fiber diameter of the fine fibers, that is, the number average particle diameter of the functional particles / the average fiber diameter of the fine fibers, is 1 to 100.
2. The flame-retardant sheet according to claim 1, wherein The number average particle size of the functional particles is 0.1 to 50 μm.
3. The flame-retardant sheet according to claim 1 or 2, wherein: The functional particles are at least one selected from the group consisting of aluminum hydroxide, titanium oxide, silica gel, zeolite, white sand ash balls, activated carbon and molecular sieves.
Citation Information
Patent Citations
Flame-retardant heat-resistant paper
JP1993230790A
Image forming device
JP2020118869A
Lightweight heat insulating molded body and method for producing the same
JP2007161561A