A single-atom catalyzed magnesium hydride solid hydrogen storage material, application and preparation method

Through the recombination of the single-atom catalyst Ni@TiO2 and magnesium hydride, the high thermodynamic stability and slow hydrogen absorption and discharge problems of MgH2 are solved, achieving more efficient hydrogen storage performance and capacity retention.

CN115784147BActive Publication Date: 2024-12-03BEIHANG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211626559.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-17
Publication Date
2024-12-03
Estimated Expiration
2042-12-17

AI Technical Summary

Technical Problem

The high thermodynamic stability of MgH2 and the slow rate of absorption and release of hydrogen limit their practical application in hydrogen storage materials, and the low atomic utilization of existing catalysts leads to loss of hydrogen storage capacity.

Method used

The single-atom catalyst Ni@TiO2 is used to load the metal single atom on TiO2 and recombinate it with magnesium hydride. The single atom catalyst is prepared by hot melt salt method, and the composite is carried out by ball milling to optimize the Ni loading and doping amount to improve MgH2 hydrogen absorption and release properties.

Benefits of technology

The initial hydrogen discharge temperature of MgH2 is significantly reduced, the hydrogen absorption and release rate and hydrogen storage density are improved, capacity loss is reduced, and the comprehensive hydrogen storage performance is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115784147B_ABST
    Figure CN115784147B_ABST
Patent Text Reader

Abstract

The present invention discloses a single-atom-catalyzed magnesium hydride solid hydrogen storage material, wherein the hydrogen storage material is composited with magnesium hydride as a main material and a catalyst, wherein the catalyst is a single-atom catalyst formed by loading a metal single atom on a carrier material. The preparation method comprises: step 1, preparing a single-atom catalyst by a hot molten salt method; step 2, compounding the single-atom catalyst and magnesium hydride to obtain the hydrogen storage material. The present invention loads a metal single atom on a carrier material to form a single-atom catalyst, and then compounds it with magnesium hydride, which can not only reduce the "dead weight" of the hydrogen storage system, but also have a strong improvement effect on the hydrogen absorption and desorption performance of MgH2.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of solid-state hydrogen storage materials of new energy materials, in particular to a single-atom catalyst composite magnesium hydride hydrogen storage material and a preparation method and application thereof. Background Art

[0002] As the basis of the current energy structure, fossil fuels have brought many new crises and challenges with their increasing demand and consumption, such as global warming and environmental pollution caused by over-exploitation of resources and excessive use of fossil fuels. Hydrogen energy is considered to be the most promising ideal alternative energy source due to its abundance, cleanliness and high energy density. However, the storage of hydrogen is still a major challenge and has become a bottleneck for the large-scale application of hydrogen energy. MgH2 has a mass hydrogen storage density of up to 7.6wt%, excellent reversibility, low cost and other advantages, making it one of the most promising hydrogen storage materials. However, MgH2 has high thermodynamic stability and high reaction energy barriers, which leads to a high dehydrogenation temperature and slow hydrogen absorption and dehydrogenation rate of MgH2, thus limiting its practical application.

[0003] In order to improve the hydrogen absorption and desorption performance of MgH2, alloying, catalysis, nano-sizing and other methods have been developed. Among them, the catalytic effect is excellent and is an effective method to improve the kinetic performance. The dehydrogenation mechanism of the Mg-TM (transition metal) system is that the multivalent transition metal participates in the reaction, promotes electron transfer, and thus accelerates the reaction. Cui [1] et al. used high-energy ball milling to prepare a series of transition metal nano-core-shell structure composites. The results of programmed temperature desorption-mass spectrometry (TPD-MS) test showed that the Mg-Ti core-shell structure nano-composite with the highest electronegativity could release hydrogen at 225°C.

[0004] However, due to the limitation of the atomic utilization of nanostructured catalysts, the part of the catalyst that is not in contact with the reactants will bring a certain amount of dead weight to the system, resulting in a loss of hydrogen storage capacity. Therefore, gradually reducing the size of the catalyst to the atomic level to achieve a "single atom catalyst" with a theoretical 100% atomic utilization is an effective way to maintain a high hydrogen storage capacity and significantly accelerate the absorption and release of hydrogen by MgH2.

[0005] So far, single-atom catalysis has been used for water splitting reactions. [2] , CO2 reduction reaction [3] , N2 reduction reaction and other electrochemical reactions, while in photocatalysis [4] and organic synthesis catalysis [5]However, single-atom catalysis for MgH2 is still a minority. After research, the inventor believes that Ni, as the most reported transition metal single atom, has an excellent catalytic effect on MgH2. At the same time, Ti is considered to be the most ideal material for catalyzing MgH2 among many transition metals. Its oxide TiO2 also performs well and has stable characteristics, and is often used as a carrier for single-atom catalysts.

[0006] References:

[0007] [1]Cui J, Liu J, Wang H, et al.Mg–TM(TM:Ti,Nb,V,Co,Mo or Ni)core–shelllike nanostructures:synthesis,hydrogen storage performance and catalyticmechanism[J].J Mater Chem A,2014,2(25):9645-55.

[0008] [2]Cheng N, Stambula S, Wang D, et al. Platinum single-atom and clustercatalysis of the hydrogen evolution reaction[J]. Nat Commun, 2016,7:13638.

[0009] [3]Mou K, Chen Z, Zhang

[0010] [4]Atomically dispersed Ni in cadmium-zinc sulfide quantum dots for high-performance visible-light photocatalytic hydrogen production[J]. 2020.

[0011] [5]Xiong Y, Sun W, Xin P, et al.Gram-Scale Synthesis of High-LoadingSingle-Atomic-Site Fe Catalysts for Effective Epoxidation of Styrene[J]. AdvMater, 2020, 32(34):e2000896. Summary of the invention

[0012] The object of the present invention is to provide a magnesium hydride hydrogen storage material composited with a single-atom catalyst and a preparation method thereof, wherein a metal single atom is loaded on a carrier material to form a single-atom catalyst, which is then composited with magnesium hydride to improve the hydrogen absorption performance of magnesium hydride and reduce capacity loss, thereby obtaining an excellent hydrogen storage composite material.

[0013] To solve the above problems, in the first aspect, an embodiment of the present invention provides a single-atom-catalyzed magnesium hydride solid-state hydrogen storage material, characterized in that the hydrogen storage material is composed of a composite of magnesium hydride as a main material and a catalyst, and the catalyst is a single-atom catalyst formed by a metal single atom loaded on a carrier material.

[0014] Furthermore, the metal single atom is one of Ni, Co, V, Nb, Mo, Zn, Fe, Ti, Cr, and Cu, and the carrier material is a metal oxide, which includes one of TiO2, Nb2O5, V2O5, Fe3O4, CeO2, SiO2, Al2O3, and ZrO2.

[0015] Furthermore, the catalyst is a single-atom catalyst Ni@TiO2 formed by single-atom Ni loaded on TiO2.

[0016] Optionally, the hydrogen storage material is prepared by ball milling a main material and a single atom catalyst; and the single atom catalyst is prepared by a hot molten salt method.

[0017] Optionally, in the single atom catalyst Ni@TiO2, the loading amount of Ni in the single atom catalyst is 1.54wt%-3.84wt%.

[0018] Optionally, the doping amount of the single atom catalyst Ni@TiO2 in the magnesium hydride hydrogen storage material is 10wt%-20wt%.

[0019] In a second aspect, an embodiment of the present invention provides a method for preparing a single-atom catalyzed magnesium hydride solid hydrogen storage material, comprising:

[0020] Step 1, preparing a single atom catalyst by a hot molten salt method;

[0021] Step 2, compounding the single atom catalyst and magnesium hydride to obtain the hydrogen storage material.

[0022] Furthermore, the preparation method comprises:

[0023] Step 1, preparation of single atom catalyst Ni@TiO2:

[0024] Through the hot molten salt method, NiCl2·6H2O, LiCl, KCl and TiO2 are uniformly mixed in a certain mass ratio and sintered. Then, the sintered product is washed and dried to obtain the single-atom catalyst Ni@TiO2.

[0025] Step 2, preparation of magnesium hydride hydrogen storage material based on single atom catalyst Ni@TiO2:

[0026] The single atom catalyst Ni@TiO2 obtained in step 1 and magnesium hydride are mixed in a certain mass ratio and then ball milled to obtain a magnesium hydride hydrogen storage material based on the single atom catalyst Ni@TiO2.

[0027] Optionally, in step 1, the mass ratio of NiCl2·6H2O to TiO2 is 0.02-0.2, and grinding is performed during mixing, and the grinding time is 15-20 minutes.

[0028] Optionally, the sintering conditions in step 1 are: under an argon protective atmosphere, the sintering temperature is 400-600° C., and the constant temperature holding time is 1-3 hours.

[0029] Optionally, in step 2, the mass ratio of the single-atom catalyst Ni@TiO2 and magnesium hydride is (10-20): (80-90); the ball milling conditions are: argon or hydrogen as the protective atmosphere, the ball-to-material ratio is 30-50, the ball milling speed is 300-500rpm, and the ball milling time is 6-10 hours.

[0030] Compared with the prior art, the present invention loads single atoms on a substrate, which can improve the hydrogen absorption performance of magnesium hydride and reduce capacity loss. In particular, in a preferred embodiment, the present invention combines two transition metal elements, Ni and Ti, and loads single atoms of Ni on a TiO2 substrate, which can not only improve the mass hydrogen storage density of the hydrogen storage system, but also produce a strong improvement effect on the hydrogen absorption and desorption performance of MgH2 through the synergistic effect of double transition metals. Specifically, the present invention uses TiO2 and NiCl2·6H2O as the main synthetic materials, adopts a hot molten salt method to prepare Ni@TiO2 single atom catalysts, and by changing the ratio of NiCl2·6H2O, different Ni@TiO2 single atom catalyst materials with Ni loading between 1.54wt% and 3.84wt% are prepared respectively. After ball milling different Ni@TiO2 materials with MgH2 and analyzing the hydrogen absorption and desorption characteristics of the composite samples by temperature programmed desorption (TPD), the results show that the Ni@TiO2 single atom catalyst prepared by the present invention can greatly improve the hydrogen absorption and desorption performance of MgH2. After conducting optimal screening of catalysts with different single-atom loadings, we found that 15 wt% Ni was added to MgH2 2.71 @TiO2 (2.71 represents the mass percentage loading of Ni in the catalyst material) After ball milling and compounding, the initial dehydrogenation temperature of the sample was reduced to 200°C. The sample can rapidly dehydrogenate at a constant temperature of 300°C, releasing 5.85wt% of hydrogen within 10 minutes, and absorbing 6.53wt% within 10 seconds at 300°C and 40bar of hydrogen pressure, further indicating that the single-atom catalyst can significantly improve the absorption and dehydrogenation kinetics of MgH2. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 Ni with different Ni single atom loadings provided in the embodiments of the present invention x @X-ray diffraction analysis (XRD) pattern of TiO2;

[0032] Figure 2 The Ni provided in the embodiment of the present invention 2.71 @Transmission electron microscope (TEM) morphology image of TiO2;

[0033] Figure 3 The Ni provided in the embodiment of the present invention 2.71 @Selected area electron diffraction (SAED) diffraction pattern of TiO2;

[0034] Figure 4 The Ni provided in the embodiment of the present invention 2.71 @TiO2 electron microscope high angle annular dark field (HAADF) dark field and X-ray spectrometer surface scanning (EDS-Mapping) image;

[0035] Figure 5 The Ni provided in the embodiment of the present invention 2.71 @XRD diffraction pattern of TiO2-MgH2;

[0036] Figure 6 The Ni provided in the embodiment of the present invention 2.71 @TEM morphology of TiO2-MgH2;

[0037] Figure 7 The Ni provided in the embodiment of the present invention 2.71 @Selected area EDS-Mapping and SAED spectrum of TiO2-MgH2;

[0038] Figure 8 Ni with different Ni single atom loadings provided in the embodiments of the present invention x @The temperature-programmed desorption (TPD) curve of MgH2 catalyzed by TiO2 (heating rate 10℃ / min);

[0039] Fig. 9 The x wt% (x=10, 15, 20) Ni provided in the embodiment of the present invention 2.71 @TPD hydrogen release diagram of TiO2-MgH2;

[0040] Fig.10 The 15wt% Ni 2.71 @Isostatic hydrogen release curve of TiO2-MgH2 at different temperatures;

[0041] Fig.11 The 15wt% Ni 2.71 @Isostatic hydrogen absorption curve of TiO2-MgH2 at different temperatures;

[0042] Fig.12 The 15wt% Ni 2.71 @Calculation results of dehydrogenation activation energy of TiO2-MgH2;

[0043] Fig.13 The 15wt% Ni 2.71 @Calculation results of hydrogen absorption activation energy of TiO2-MgH2;

[0044] Fig.14 The 15wt% Ni 2.71 @TiO2-MgH2 hydrogen absorption and desorption cycle test diagram. DETAILED DESCRIPTION

[0045] The principles and measures of the present invention will be described below with reference to several exemplary embodiments given in the accompanying drawings. It should be understood that these embodiments are described only to enable those skilled in the art to better understand and implement the present invention, and are not intended to limit the scope of the present invention in any way.

[0046] The embodiment of the present invention provides a method for preparing a magnesium hydride hydrogen storage material composited with a single-atom catalyst, wherein TiO2 and NiCl2·6H2O are used as the main synthetic materials, and a hot molten salt method is used to prepare a Ni@TiO2 single-atom catalyst. After the catalyst is synthesized, it is composited with MgH2 by ball milling, and the optimal screening of catalysts with different single-atom loadings and doping amounts and in-depth hydrogen storage performance testing are performed.

[0047] Example 1

[0048] <Preparation of single-atom catalysts>

[0049] In one embodiment, the specific synthesis method is as follows: first weigh 20 mg NiCl2·6H2O, 0.9 g LiCl, 1.1 g KCl and 1 g TiO2, and grind them in an agate mortar for 10 min to ensure uniform mixing of the above materials. Then transfer the mixed sample to an alumina crucible and place it in a tubular furnace for sintering. The tubular furnace is always fed with an N2 inert atmosphere during operation, and is ventilated for 15 min before heating to ensure that the air in the furnace tube is completely exhausted. The heating rate of the tubular furnace is 10°C / min, and it is maintained at a temperature of 500°C for 2 hours. After the tubular furnace is cooled to room temperature, take out the sample and place it in a centrifuge tube, add 15 ml of deionized water for washing and centrifuge at 5000 rpm for 3 minutes, pour out the supernatant, and continue to add 15 ml of deionized water to wash the precipitate again. This process was repeated three times to wash away the salt (LiCl and KCl) in the sample, and finally the precipitated sample in the centrifuge tube was dried in a forced air oven at 80°C overnight to obtain the final single atom catalyst Ni@TiO2.

[0050] <Preparation of Hydrogen Storage Materials>

[0051] The single atom catalyst was ball-milled with MgH2 to obtain a composite material, and the mass ratio of Ni@TiO2 to magnesium hydride was 10:90. The ball milling conditions were: argon as the protective atmosphere, the ball-to-powder ratio was 40:1, the ball milling speed was 400 rpm, and in order to reduce the high temperature generated during the high-energy ball milling process, the ball milling program was set accordingly, and the operation mode of resting for 5 minutes after each ball milling was set, and the actual total ball milling time was 8 hours.

[0052] Example 2

[0053] <Preparation of single-atom catalysts>

[0054] In one embodiment, the specific synthesis method is as follows: first weigh 50 mg NiCl2·6H2O, 0.9 g LiCl, 1.1 g KCl and 1 g TiO2, and grind them for 15 min in an agate mortar to ensure uniform mixing of the above materials. Then transfer the mixed sample to an alumina crucible and place it in a tubular furnace for sintering. The tubular furnace is always fed with an N2 inert atmosphere during operation, and is ventilated for 15 min before heating to ensure that the air in the furnace tube is completely exhausted. The heating rate of the tubular furnace is 10°C / min, and it is maintained at a temperature of 400°C for 3 hours. After the tubular furnace is cooled to room temperature, take out the sample and place it in a centrifuge tube, add 15 ml of deionized water for washing and centrifuge at 5000 rpm for 3 minutes, pour out the supernatant, and continue to add 15 ml of deionized water to wash the precipitate again. This process was repeated three times to wash away the salt (LiCl and KCl) in the sample, and finally the precipitated sample in the centrifuge tube was dried in a forced air oven at 80°C overnight to obtain the final single atom catalyst Ni@TiO2.

[0055] <Preparation of Hydrogen Storage Materials>

[0056] The single atom catalyst was ball-milled with MgH2 to obtain a composite material. The mass ratio of Ni@TiO2 and magnesium hydride was 20:80. The ball-milling conditions were: argon as the protective atmosphere, the ball-to-powder ratio was 50:1, the ball-milling speed was 300 rpm, and in order to reduce the high temperature generated during the high-energy ball milling process, the ball mill operation program was set accordingly, and an operation mode of resting for 5 minutes after each ball milling was set. The actual total ball milling time was 6 hours.

[0057] Example 3

[0058] <Preparation of single-atom catalysts>

[0059] In one embodiment, the specific synthesis method is as follows: first weigh 150 mg NiCl2·6H2O, 0.9 g LiCl, 1.1 g KCl and 1 g TiO2, and grind them in an agate mortar for 20 min to ensure uniform mixing of the above materials. Then transfer the mixed sample to an alumina crucible and place it in a tubular furnace for sintering. The tubular furnace is always ventilated with an Ar inert atmosphere during operation, and ventilated for 15 min before heating to ensure that the air in the furnace tube is completely exhausted. The heating rate of the tubular furnace is 10 ° C / min, and it is maintained at a temperature of 600 ° C for 1 hour. After the tubular furnace is cooled to room temperature, take out the sample and place it in a centrifuge tube, add 15 ml of deionized water for washing and centrifuge at 5000 rpm for 3 minutes, pour out the supernatant, and continue to add 15 ml of deionized water to wash the precipitate again. This process was repeated three times to wash away the salt (LiCl and KCl) in the sample, and finally the precipitated sample in the centrifuge tube was dried in a forced air oven at 80°C overnight to obtain the final single atom catalyst Ni@TiO2.

[0060] <Preparation of Hydrogen Storage Materials>

[0061] The single atom catalyst was ball-milled with MgH2 to obtain a composite material. The mass ratio of Ni@TiO2 and magnesium hydride was 15:85. The ball milling conditions were: argon as the protective atmosphere, the ball-to-powder ratio was 30:1, the ball milling speed was 500 rpm, and in order to reduce the high temperature generated during the high-energy ball milling process, the ball mill operation program was set accordingly, and an operation mode of resting for 5 minutes after each ball milling was set. The actual total ball milling time was 10 hours.

[0062] Example 4

[0063] In this example, 100 mg of NiCl2·6H2O is used as the raw material, and the other preparation parameters are the same as those in Example 1.

[0064] Example 5

[0065] In this embodiment, 100 mg of NiCl2·6H2O is used as the raw material, the mass ratio of the single-atom catalyst Ni@TiO2 and magnesium hydride is 20:80, and the other preparation parameters are the same as those in Example 1.

[0066] Example 6

[0067] In this embodiment, 100 mg of NiCl2·6H2O is used as the raw material, the mass ratio of the single-atom catalyst Ni@TiO2 and magnesium hydride is 15:85, and the other preparation parameters are the same as those in Example 1.

[0068] Example 7

[0069] In this example, 200 mg of NiCl2·6H2O is used as the raw material, and the other preparation parameters are the same as those in Example 1.

[0070] In the above embodiments, NiCl2·6H2O was increased to 2.5, 5, 7.5 and 10 times, and Ni@TiO2 samples with different Ni doping amounts of 250%, 500%, 750% and 1000% were prepared according to the above preparation process. The samples synthesized from the above 100%-1000% Ni precursor were characterized by inductively coupled plasma mass spectrometry (ICP-MS), and the actual Ni loading amounts were measured to be 1.54wt%, 2.06wt%, 2.71wt%, 3.26wt%, 3.84wt%, respectively, so we named them Ni@TiO2, ... 1.54 @TiO2、Ni 2.06 @TiO2、Ni 2.71 @TiO2、Ni 3.84 @TiO2、Ni 3.26 @TiO2.

[0071] <Catalyst Characterization>

[0072] By x @TiO2 was subjected to XRD characterization, and the characterization results are as follows Figure 1 As shown, it can be seen that each sample has three obvious diffraction peaks at 2θ=25.3°, 38.2° and 48.2°, which is consistent with the TiO2 anatase spectrum. However, no diffraction peak of Ni single substance was observed. Since ICP contains Ni element, but XRD characterization did not detect the presence of Ni, this also indirectly indicates that we have synthesized Ni@TiO2, a sample in which Ni single atoms are highly dispersed in TiO2, by controllably adjusting the doping ratio of the precursor through the hot molten salt method.

[0073] Combined with the subsequent catalytic effect, the best Ni 2.71 @TiO2, the catalyst samples were characterized by TEM, as shown in the attached Figure 2 The measured distance between the lattice fringes is d = 0.3611nm, which is consistent with the lattice spacing of the TiO2 (101) crystal plane, proving that the main load of the sample is TiO2. 2.71 @TiO2 contains single-atom Ni. The present invention characterized the sample by dark-field HAADF and X-ray energy dispersive spectroscopy (EDS) using a spherical aberration-corrected transmission microscope. Figure 3 As shown. Since Ni has a larger atomic number than Ti, it appears brighter under HAADF dark field imaging. Figure 4As shown in the yellow circle in the middle, it can be clearly observed that there are some obvious bright spots on the substrate material. Combined with the EDS-Mapping image, it shows that the bright spots on the TiO2 surface are highly dispersed Ni single atoms, indicating that a catalyst with single-atom Ni dispersed in TiO2 has been successfully prepared.

[0074] <Preparation of Hydrogen Storage Materials>

[0075] In this embodiment, the catalyst and MgH2 are ball-milled to obtain a composite material. In a glove box filled with Ar gas, single-atom catalyst Ni@TiO2 with different Ni doping amounts is first compounded with MgH2 at a mass ratio of 15wt%, and Ni is selected. 2.71 @TiO2 is the best catalyst, and then Ni 2.71 @TiO2 is compounded with MgH2 in a mass ratio of 10wt%, 15wt%, and 20wt% (i.e., Ni@TiO2 accounts for 10wt%, 15wt%, and 20wt% of the total mass of Ni@TiO2 and MgH2), so as to select the optimal doping amount.

[0076] <Characterization of Hydrogen Storage Materials>

[0077] To confirm with Ni 2.71 The phase composition of the material after ball milling of the composite material of @TiO2 and MgH2 was characterized by XRD in this patent, as shown in the attached Figure 5 As shown, Ni 2.71 The XRD pattern of the @TiO2-MgH2 sample is mainly MgH2, and there is a slight bulge at 25.3°, which can be compared with Ni 2.71 @TiO2 single atom catalyst. This is because only 15wt% Ni was introduced into the system. 2.71 @TiO2 single atom catalyst material, so the diffraction peak of the catalyst is on Ni 2.71 The XRD spectrum of @TiO2-MgH2 is weak. No other diffraction peaks were observed, indicating that no additional side reactions occurred during the ball milling process to generate other impurities. The grain size of MgH2 in the sample was calculated to be 29nm using the Scherrer formula.

[0078] After determining Ni 2.71 @TiO2-MgH2, we also performed spherical aberration-corrected transmission electron microscopy on the sample to obtain Ni 2.71 @TiO2-MgH2 morphology, observation and analysis of sample Ni 2.71 @The distribution of TiO2 single atom catalyst on MgH2. Figure 6As can be seen from part (a), the morphology of the sample is superimposed on each other and the surface is wrinkled. Such a structure can help magnesium hydride shorten the diffusion channel of hydrogen during the dehydrogenation process, help the rapid diffusion of hydrogen, and thus improve the kinetics of hydrogen absorption and dehydrogenation. In order to observe the surface distribution of the sample more clearly, we further increase the magnification of the electron microscope and observe the surface of the sample from the attached image. Figure 6 In part (b), it can be clearly seen that there is a clear boundary in the distribution of the three materials on the sample surface. By measuring the crystal plane spacing d = 0.2575nm, 0.2303nm, and 0.1925nm in the image, they can correspond to the (101) crystal plane orientation of MgH2, and the (004) and (200) crystal plane orientations of TiO2, respectively. This also corresponds to the diffraction characteristic peaks of the sample's XRD spectrum. However, it is worth mentioning that in the electron microscope image we measured a crystal plane spacing of d = 0.2080nm. By comparison, we found that this belongs to the MgO (020) crystal plane orientation. The reason is that we exposed the sample to the air when the slide was equipped before the TEM test, and the MgH2 in the sample reacted with the water and oxygen in the air to generate MgO. Similarly, Ni 2.71 @The embedding of TiO2 single-atom catalyst on the surface of MgH2 can hinder the agglomeration of MgH2 nanoparticles to a certain extent in the subsequent hydrogen absorption and desorption process, thereby continuously improving its hydrogen absorption and desorption properties.

[0079] During the TEM test, the present invention also tests Ni 2.71 @ TiO2-MgH2 samples were subjected to EDS-Mapping. Figure 7 It can be seen that in the selected scanning area, there is a whole TiO2 nanoparticle, while in other areas, TiO2 is evenly distributed in the area where the Mg element is located. This also shows that this paper has achieved Ni 2.71 @Uniform composite of TiO2 single atom catalyst and MgH2. And from the final comprehensive scanning synthesis diagram of all elements, it can be seen that due to the stacked structure of MgH2, the TiO2 particles are just loaded on the surface of the bottom MgH2. This structure can play the role of hydrogen pump of the catalyst, promote the electron transfer in the process of hydrogen absorption and desorption, and thus improve the hydrogen absorption and desorption characteristics. In addition, we can also see that the Ni element is evenly distributed in the entire scanning area, and the synergistic catalytic effect of the transition elements Ni and Ti can help MgH2 achieve better hydrogen absorption and desorption effects.

[0080] In addition, the present invention also performs SAED characterization on the samples in this area, calibrates the crystal structure of the material by the electron diffraction spots in SAED, and by corresponding the values ​​of the measured diffraction rings with the diffraction ring data of the standard material one by one, it is found that the substances measured by SAED correspond to the (101) crystal plane of TiO2, the (101) crystal plane of MgH2, the (111) crystal plane of MgO, the (020) crystal plane of MgO and the (200) crystal plane of TiO2, respectively, confirming that the main composition of the material in the scanning area is TiO2, MgH2 and MgO.

[0081] <Hydrogen Desorption Performance>

[0082] In terms of hydrogen release temperature, the prepared Ni@TiO2 and MgH2 were ball-milled and composited in this embodiment, and commercial TiO2 and pure MgH2 were selected as control groups. TPD temperature-dependent hydrogen release tests were performed on each sample, and the results are shown in the attached figure. Figure 8 As shown. The MgH2 sample doped with commercial TiO2 as a catalyst has a significantly lower dehydrogenation temperature than that of undoped MgH2. This group of samples can start to dehydrogenate at around 250°C, which is nearly 100°C lower than the dehydrogenation temperature of undoped MgH2. However, its dehydrogenation rate is relatively slow, and it continues to dehydrogenate during the process of heating to 400°C, and finally reaches a final dehydrogenation amount of 5.97wt% at 400°C. When Ni@TiO2 is introduced into MgH2, the material exhibits a lower dehydrogenation temperature and faster dehydrogenation rate than when ordinary TiO2 is introduced. Among them, Ni 2.71 @TiO2 in Ni x @TiO2 (x = 1.54, 2.06, 2.54, 2.71, 3, 26, 3.84) has the best catalytic effect. Figure 8 It can be seen that Ni 2.71 The initial dehydrogenation temperature of the @TiO2-MgH2 composite material was reduced to 200°C, and a total of 6.56wt% of hydrogen could be released within 18 minutes. The sample showed the lowest dehydrogenation temperature, the highest dehydrogenation rate and the largest dehydrogenation amount. The above experimental results show that the single-atom catalyst Ni@TiO2 developed by the present invention can not only significantly improve the kinetic characteristics of hydrogen absorption and dehydrogenation of MgH2, but also effectively prevent the loss of MgH2 hydrogen storage capacity during ball milling, thereby achieving better comprehensive hydrogen storage performance.

[0083] The present invention is preferably the best catalyst Ni 2.71 @TiO2, in order to study the different doping amounts of Ni 2.71 The effect of @TiO2 catalyst on the dehydrogenation performance of MgH2 was further prepared by x wt% Ni 2.71@TiO2-MgH2 (where x = 10, 15, 20) composite materials were tested for TPD temperature-dependent hydrogen release. The experimental results are shown in the attached Fig. 9 As shown, 15wt% Ni 2.71 @TiO2 performs best, showing x @TiO2 and the best hydrogen release performance at different doping levels, so the embodiment of the present invention selects 15wt%-Ni 2.71 @TiO2-MgH2 conducts more in-depth hydrogen absorption and desorption tests under constant temperature conditions.

[0084] <Hydrogen absorption and desorption kinetics test>

[0085] In terms of hydrogen absorption and desorption kinetics, for the preferred 15wt% Ni 2.71 @TiO2-MgH2 material, constant temperature hydrogen absorption and desorption tests were carried out at different temperatures ( Fig.10 , 11 ), and the corresponding hydrogen absorption and desorption activation energy calculations are performed ( Fig.12 , 13 ). The Arrhenius formula was used for fitting calculation, and the activation energy of hydrogen release was 133.16KJ / mol H2, and the activation energy of hydrogen absorption was Ea=35.2KJ / mol H2. Compared with the theoretical dehydrogenation activation energy of MgH2 of 160kJ / mol H2 and the theoretical hydrogen absorption activation energy of 87.3KJ / mol H2, both are significantly lower, indicating that 15wt% Ni 2.71 @TiO2 greatly improves the hydrogen absorption and desorption kinetics of MgH2.

[0086] <Cyclic performance test>

[0087] In terms of hydrogen absorption and desorption cycle performance, the 15wt% Ni 2.71 @TiO2-MgH2 was subjected to a constant temperature hydrogen absorption and desorption cycle test at 300°C. The results are as follows Fig.14 At this temperature, the material exhibits excellent hydrogen absorption and desorption performance. The dehydrogenated sample can reach hydrogen absorption saturation within 20 seconds. The first hydrogen desorption amount of the sample is 5.67wt%. After 10 reversible cycles of hydrogen absorption and desorption, 15wt%-Ni 2.71 @The capacity of the TiO2-MgH2 sample is still 5.33wt%, showing relatively excellent cycle stability performance and relatively stable cycle durability.

[0088] From the above experimental results, it can be seen that the embodiment of the present invention gradually reduces the size of the catalyst to the atomic level, thereby achieving a "single atom catalyst" with 100% catalyst atom utilization rate, which can effectively improve the hydrogen storage performance of MgH2. For example, when the doping amount of the single atom catalyst Ni@TiO2 is 15wt%, the initial dehydrogenation temperature of the system drops to 200°C, and the dehydrogenation amount reaches 6.56wt%. It can be inferred that it has a strong anti-oxidation effect on MgH2. The system can achieve rapid dehydrogenation at a constant temperature of 300°C, and the dehydrogenation amount reaches 5.85wt% within 10 minutes; when absorbing hydrogen at a constant temperature of 300°C, it can achieve rapid dehydrogenation with a content of 6.53wt% within 10 seconds. As the control group, the pure magnesium hydride has a hydrogen desorption capacity of 7.07wt% after the ball milling process, while the magnesium hydride doped with a certain amount of Ni@TiO2 single atom catalyst can completely dehydrogenate after deducting the mass of the catalyst in the system, reaching a dehydrogenation amount of 7.6wt%. That is, the prepared Ni@TiO2 single-atom catalyst can achieve good protection for magnesium hydride to a certain extent, avoiding the loss of hydrogen storage capacity during the ball milling process.

[0089] The invention concept is described in detail using specific examples herein, and the description of the above embodiments is only used to help understand the core idea of ​​the invention. It should be pointed out that any obvious modification, equivalent substitution or other improvement made by a person of ordinary skill in the art without departing from the invention concept should be included in the protection scope of the present invention.

Claims

1. A single-atom catalyzed magnesium hydride solid hydrogen storage material, characterized in that: The hydrogen storage material is composited with magnesium hydride as a main material and a catalyst. The catalyst is a single-atom catalyst Ni@TiO2 formed by single-atom Ni loaded on TiO2. The loading amount of Ni in the single-atom catalyst is 1.54wt%-3.84wt%.

2. The single-atom catalyzed magnesium hydride solid hydrogen storage material according to claim 1, characterized in that: The doping amount of the single atom catalyst Ni@TiO2 in the magnesium hydride hydrogen storage material is 10 wt %-20 wt %.

3. Application of single-atom catalyst in improving the hydrogen storage performance of magnesium hydride, characterized in that: The catalyst is a single-atom catalyst Ni@TiO2 formed by loading single-atom Ni on TiO2, and the loading amount of Ni in the single-atom catalyst is 1.54wt%-3.84wt%.

4. A method for preparing the single-atom catalyzed magnesium hydride solid hydrogen storage material according to claim 1, characterized in that: include Step 1, preparing a single atom catalyst by a hot molten salt method; Step 2, compounding the single atom catalyst and magnesium hydride to obtain the hydrogen storage material; Step 1 includes: By using a hot molten salt method, NiCl2·6H2O, LiCl, KCl and TiO2 are uniformly mixed in a certain mass ratio and sintered. The sintered product is then washed and dried to obtain the single-atom catalyst Ni@TiO2. Step 2 includes: The single-atom catalyst Ni@TiO2 obtained in step 1 and magnesium hydride are mixed in a certain mass ratio and then ball-milled to obtain a magnesium hydride hydrogen storage material based on the single-atom catalyst Ni@TiO2; The sintering conditions in step 1 are: under an argon protective atmosphere, the sintering temperature is 400-600° C., and the constant temperature holding time is 1-3 hours.

5. The preparation method according to claim 4, characterized in that: In the step 1, the mass ratio of NiCl2·6H2O to TiO2 is 0.02-0.2, and grinding is performed during mixing, and the grinding time is 15-20 minutes.

6. The preparation method according to claim 4, characterized in that: In the step 2, the mass ratio of the single-atom catalyst Ni@TiO2 and magnesium hydride is (10-20): (80-90); the ball milling conditions are: argon or hydrogen as the protective atmosphere, the ball-to-material ratio is 30-50, the ball milling speed is 300-500rpm, and the ball milling time is 6-10 hours.