A pattern electroplating process and printed circuit board

By using pulse plating in the graphics electroplating process to adjust the current density and pulse width ratio, the problem of high line arc rate is solved, and lower arc rate and higher electrical reliability is achieved.

CN115787016BActive Publication Date: 2024-11-26上海天承化学有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211614783.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-14
Publication Date
2024-11-26
Estimated Expiration
2042-12-14

AI Technical Summary

Technical Problem

In the existing graphic electroplating process, the arc rate of the lines is relatively high, making it difficult to achieve an ideal rectangular shape, which affects electrical reliability and line density.

Method used

The pulse plating process is adopted to reduce the plating tip effect and reduce the arc rate of the line by defining the current density ratio and pulse width ratio of the forward pulse and the reverse pulse. Specific measures include at least one segment of pulse plating in the graphical plating process. Each segment of pulse plating includes repeated forward pulses and reverse pulses. The ratio of the current density of the forward pulse to the current density of the reverse pulse is 1: (0.3~ 3) The ratio of the pulse width of the forward pulse to the pulse width of the reverse pulse is greater than or equal to 20:1.

Benefits of technology

The arc rate of the line is effectively reduced, reaching less than 17%, approaching the ideal rectangular shape, and improving electrical reliability and line density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115787016B_ABST
    Figure CN115787016B_ABST
Patent Text Reader

Abstract

The present invention provides a pattern electroplating process and a printed circuit board, wherein the pattern electroplating process includes at least one pulse electroplating of the circuit board in a plating solution, each pulse electroplating includes repeated forward pulses and reverse pulses; the ratio of the current density of the forward pulse to the current density of the reverse pulse is 1:(0.3-3); the ratio of the pulse width of the forward pulse to the pulse width of the reverse pulse is greater than or equal to 20:1. In the present invention, by limiting the ratio of the current density of the forward pulse to the current density of the reverse pulse and the ratio of the pulse width of the forward pulse to the pulse width of the reverse pulse, the problem of high arc rate of the circuit caused by the electroplating tip effect is weakened; the arc rate of the circuit obtained by the pattern electroplating process provided by the present invention is low, reaching less than 17%, presenting a rectangle that is more inclined to the ideal state.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electroplating, and relates to a pattern electroplating process, and in particular to a pattern electroplating process and a printed circuit board. Background Art

[0002] As electronic devices develop towards being lighter, thinner, shorter and smaller, printed circuit boards are also required to be lighter and thinner, mainly in terms of increasingly dense lines, smaller line widths and line spacings, high-density connections, and stronger electrical reliability. Especially for express circuit board manufacturers, the requirements for lightness and thinness are particularly prominent. As a manufacturing process, graphic electroplating is an important process for thickening the circuit layer and hole plating after external light imaging.

[0003] The ideal shape of the circuit after electroplating in the graphic electroplating process is a rectangle, but in reality, the circuit after electroplating will have a certain curvature, which is called the arc rate of the circuit. The arc rate of the circuit in the graphic electroplating process is a key and challenging indicator. In order to achieve a good graphic electroplating effect, it is necessary to try to reduce the arc rate of the circuit. At present, the arc rate of the circuit of the substrate electroplating is required to be ≤20%.

[0004] CN112752447A discloses a manufacturing process for embedded component circuit boards. The inner core board after drilling is subjected to plasma degumming treatment to remove residual glue residue, and there will be no gluing process to prevent board surface pollution. The inner core board is then subjected to board electrical treatment to improve the physical properties of the coating and increase the copper plating deposition rate. The copper surface and the inner core board substrate surface are both roughened to prevent delamination and increase surface bonding. Specific pattern electroplating process parameters are used to ensure that the plating solution has good dispersion ability and ductility, and to ensure the brightness of the coating. However, the arc rate of the circuit after pattern electroplating in this embedded component circuit board manufacturing process is relatively high.

[0005] CN103118495A discloses a PCB board manufacturing process, including the following steps: (1) following the conventional PCB board manufacturing process to the dry film pasting step before pattern electroplating; (2) when making a film, the board edge reserved according to the process requirements is used as an edge sealing area, and the edge sealing area is made into a light-transmitting area on the film; (3) the edge sealing area is coated by exposure and development; (4) the developed PCB board is subjected to pattern electroplating according to the designed electroplating process; (5) the PCB board after pattern electroplating is subjected to film stripping and post-processing. Similarly, the arc rate of the circuit after pattern electroplating in the PCB board manufacturing process is relatively high.

[0006] The currently disclosed pattern electroplating processes all have certain defects, and there is a problem that the arc rate of the circuit after pattern electroplating is high. Therefore, it is very important to develop and design a new type of pattern electroplating process. Summary of the invention

[0007] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a pattern electroplating process and a printed circuit board. In the present invention, the pattern electroplating process adopts pulse electroplating. During the forward pulse, due to the existence of the tip effect, the deposition speed of the metal in the middle of the circuit is faster; during the reverse pulse, the dissolution speed of the metal in the middle of the circuit is faster, thereby weakening the tip effect of electroplating; in the present invention, by limiting the ratio of the current density of the forward pulse to the current density of the reverse pulse and the ratio of the pulse width of the forward pulse to the pulse width of the reverse pulse, the problem of the high arc rate of the circuit caused by the electroplating tip effect is weakened; the arc rate of the circuit obtained by the pattern electroplating process provided by the present invention is relatively low, reaching less than 17%, presenting a rectangle that is more inclined to the ideal state.

[0008] To achieve this object, the present invention adopts the following technical solutions:

[0009] In a first aspect, the present invention provides a pattern electroplating process, the pattern electroplating process comprising performing at least one pulse electroplating of a circuit board in a plating solution, each pulse electroplating comprising a forward pulse and a reverse pulse repeated in sequence;

[0010] The ratio of the current density of the forward pulse to the current density of the reverse pulse is 1:(0.3-3);

[0011] The ratio of the pulse width of the forward pulse to the pulse width of the reverse pulse is greater than or equal to 20:1.

[0012] Since the circuits of graphic electroplating are relatively small, the current distribution is disturbed by the dry film, and the current distribution at the edge of the dry film is relatively small, resulting in a tip effect of electroplating during the electroplating process. Therefore, the use of DC electroplating in the graphic electroplating process will cause a higher arc rate of the circuit.

[0013] The pattern electroplating process of the present invention adopts pulse electroplating. Due to the existence of the tip effect during the forward pulse, the deposition speed of the metal in the middle of the circuit is faster; during the reverse pulse, the dissolution speed of the metal in the middle of the circuit is faster, thereby weakening the tip effect of the electroplating; the present invention reduces the problem of high arc rate of the circuit caused by the electroplating tip effect by limiting the ratio of the current density of the forward pulse to the current density of the reverse pulse and the ratio of the pulse width of the forward pulse to the pulse width of the reverse pulse; the arc rate of the circuit obtained by the pattern electroplating process provided by the present invention is relatively low, reaching less than 17%, and presenting a rectangle that is more inclined to the ideal state.

[0014] The present invention limits the ratio of the current density of the forward pulse to the current density of the reverse pulse to 1:(0.3-3), for example, it can be 1:0.3, 1:0.4, 1:0.5, 1:0.7, 1:1, 1:1.2, 1:1.5, 1:1.7, 1:2, 1:2.2, 1:2.5, 1:2.7 or 1:3, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0015] The present invention limits the ratio of the pulse width of the forward pulse to the pulse width of the reverse pulse to be greater than or equal to 20:1, for example, it can be 20:1, 22:1, 25:1, 27:1, 30:1, 32:1, 35:1, 37:1, 40:1, 45:1, 50:1 or 60:1, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0016] Preferably, the current density of the forward pulse is 10-25ASF, for example, it can be 10ASF, 12ASF, 14ASF, 16ASF, 18ASF, 20ASF, 22ASF, 24ASF or 25ASF, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0017] Preferably, the pulse width of the forward pulse is 20 to 60 ms, for example, it can be 20ms, 25ms, 30ms, 35ms, 40ms, 45ms, 50ms, 55ms or 60ms, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0018] Preferably, the current density of the reverse pulse is 2.5-66ASF, for example, it can be 2.5ASF, 5ASF, 2.5ASF, 10ASF, 15ASF, 20ASF, 25ASF, 30ASF, 35ASF, 40ASF, 45ASF, 50ASF, 55ASF, 60ASF, 65ASF or 66ASF, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0019] Preferably, the pulse width of the reverse pulse is 0.5 to 2 ms, for example, it can be 0.5ms, 0.6ms, 0.7ms, 0.8ms, 0.9ms, 1ms, 1.1ms, 1.2ms, 1.3ms, 1.4ms, 1.5ms, 1.6ms, 1.7ms, 1.8ms, 1.9ms or 2ms, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0020] Preferably, the pattern electroplating process further includes at least one section of direct current electroplating.

[0021] Preferably, the current density of each section of the direct current plating is 8 to 22ASF, for example, it can be 8ASF, 9ASF, 10ASF, 11ASF, 12ASF, 13ASF, 14ASF, 15ASF, 16ASF, 17ASF, 18ASF, 19ASF, 20ASF, 21ASF or 22ASF, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0022] Preferably, the ratio of the total time of pulse plating to the total time of DC plating in the graphic electroplating process is 1:(0.5-2), for example, it can be 1:0.5, 1:0.7, 1:0.9, 1:1, 1:1.2, 1:1.4, 1:1.6, 1:1.8 or 1:2, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0023] Preferably, the total time of the graphic electroplating process is 50 to 120 minutes, for example, it can be 50 minutes, 60 minutes, 70 minutes, 80 minutes, 90 minutes, 100 minutes, 110 minutes or 120 minutes, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0024] Preferably, the distance between the cathode and the anode in the graphic electroplating process is 150 to 250 mm, for example, it can be 150 mm, 160 mm, 170 mm, 180 mm, 190 mm, 200 mm, 210 mm, 220 mm, 230 mm, 240 mm or 250 mm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0025] Preferably, the temperature of the plating solution in the graphic electroplating process is 22-28°C, for example, it can be 22°C, 23°C, 24°C, 25°C, 26°C, 27°C or 28°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0026] Preferably, the plating solution comprises a copper plating solution.

[0027] Preferably, the solute of the copper plating solution includes a copper source, concentrated sulfuric acid and a chlorine source.

[0028] The solvent of the copper plating solution of the present invention comprises water, and the mass fraction of the concentrated sulfuric acid is 98wt%.

[0029] Preferably, the copper source includes any one of copper oxide, copper hydroxide or copper salt, or a combination of at least two thereof. Typical but non-limiting combinations include a combination of copper oxide and copper hydroxide, a combination of copper hydroxide and a copper salt, a combination of copper oxide and a copper salt, or a combination of copper oxide, copper hydroxide and a copper salt.

[0030] Preferably, the copper salt comprises any one of copper sulfate, copper nitrate or copper chloride or a combination of at least two thereof, and typical but non-limiting combinations include a combination of copper sulfate and copper nitrate, a combination of copper nitrate and copper chloride, or a combination of copper sulfate, copper nitrate and copper chloride.

[0031] Preferably, the chlorine source comprises sodium chloride and / or potassium chloride.

[0032] Preferably, the concentration of the copper source is 240-280 g / L, for example, 240 g / L, 245 g / L, 250 g / L, 255 g / L, 260 g / L, 265 g / L, 270 g / L, 275 g / L or 280 g / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0033] Preferably, the concentration of the concentrated sulfuric acid is 50-100 g / L, for example, 50 g / L, 55 g / L, 60 g / L, 65 g / L, 70 g / L, 75 g / L, 80 g / L, 85 g / L, 90 g / L, 95 g / L or 100 g / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0034] Preferably, the concentration of the chlorine source is 45-70 ppm, for example, 45 ppm, 50 ppm, 55 ppm, 60 ppm, 65 ppm or 70 ppm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0035] As a preferred technical solution of the pattern electroplating process described in the first aspect, the pattern electroplating process includes performing at least one section of direct current electroplating and at least one section of pulse electroplating on the circuit board in a plating solution;

[0036] The current density of the direct current plating in each section is 8-22 ASF;

[0037] Each section of the pulse plating includes a forward pulse and a reverse pulse that are repeated in sequence, the current density of the forward pulse is 10-25 ASF, the pulse width of the forward pulse is 20-60 ms, the current density of the reverse pulse is 2.5-66 ASF, and the pulse width of the reverse pulse is 0.5-2 ms;

[0038] The total time of the pattern electroplating process is 50 to 120 minutes, and the ratio of the total time of pulse electroplating to the total time of DC electroplating is 1:(0.5 to 2);

[0039] In the pattern electroplating process, the distance between the cathode and the anode is 150-250 mm, and the temperature of the plating solution is 22-28°C.

[0040] In a second aspect, the present invention provides a printed circuit board, which is obtained by the pattern electroplating process described in the first aspect, and the arc rate of the circuit of the printed circuit board is less than or equal to 17%.

[0041] Compared with the prior art, the present invention has the following beneficial effects:

[0042] The pattern electroplating process of the present invention adopts pulse electroplating. Due to the existence of the tip effect during the forward pulse, the deposition speed of the metal in the middle of the circuit is faster; during the reverse pulse, the dissolution speed of the metal in the middle of the circuit is faster, thereby weakening the tip effect of the electroplating; the present invention reduces the problem of high arc rate of the circuit caused by the electroplating tip effect by limiting the ratio of the current density of the forward pulse to the current density of the reverse pulse and the ratio of the pulse width of the forward pulse to the pulse width of the reverse pulse; the arc rate of the circuit obtained by the pattern electroplating process provided by the present invention is relatively low, reaching less than 17%, and presenting a rectangle that is more inclined to the ideal state. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 This is a circuit diagram obtained by the pattern electroplating process in Example 1 of the present invention.

[0044] Figure 2 This is a circuit diagram obtained by the pattern electroplating process in Example 3 of the present invention.

[0045] Figure 3 This is a circuit diagram obtained by the pattern electroplating process in Example 4 of the present invention.

[0046] Figure 4 This is the circuit diagram obtained by the graphic electroplating process in Comparative Example 4 of the present invention. DETAILED DESCRIPTION

[0047] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0048] Example 1

[0049] This embodiment provides a pattern electroplating process, wherein the pattern electroplating process is to perform a pulse electroplating on the circuit board in a plating solution, wherein the pulse electroplating includes repeating a forward pulse and a reverse pulse in sequence;

[0050] The current density of the forward pulse is 20ASF and the pulse width is 40ms, and the current density of the reverse pulse is 25ASF and the pulse width is 1ms;

[0051] The total time of the pattern electroplating process, i.e. the time of pulse electroplating, is 80 minutes;

[0052] In the pattern electroplating process, the distance between the cathode and the anode is 200 mm, and the temperature of the plating solution is 25°C;

[0053] The solutes of the plating solution include: copper sulfate pentahydrate with a concentration of 250 g / L, 98 wt% concentrated sulfuric acid with a concentration of 80 g / L, and sodium chloride with a concentration of 50 ppm, and the solvent is water.

[0054] Example 2

[0055] This embodiment provides a pattern electroplating process, which includes performing three-stage pulse electroplating on a circuit board in a plating solution, each stage of pulse electroplating including repeated forward pulses and reverse pulses;

[0056] The first pulse plating:

[0057] The current density of the forward pulse is 10ASF, the pulse width is 60ms, the current density of the reverse pulse is 3ASF, the pulse width is 2ms, and the time of the first pulse plating is 30min;

[0058] The second pulse plating:

[0059] The current density of the forward pulse is 15ASF, the pulse width is 20ms, the current density of the reverse pulse is 45ASF, the pulse width is 0.5ms, and the second pulse plating time is 10min;

[0060] The third pulse plating:

[0061] The current density of the forward pulse is 25ASF, the pulse width is 30ms, the current density of the reverse pulse is 66ASF, the pulse width is 1.2ms, and the third pulse plating time is 10min;

[0062] In the pattern electroplating process, the distance between the cathode and the anode is 150 mm, and the temperature of the plating solution is 28° C.

[0063] The solutes of the plating solution include: copper sulfate pentahydrate with a concentration of 280 g / L, 98 wt% concentrated sulfuric acid with a concentration of 50 g / L, and potassium chloride with a concentration of 60 ppm, and the solvent is water.

[0064] Example 3

[0065] This embodiment provides a pattern electroplating process, which includes a section of direct current electroplating and a section of pulse electroplating performed sequentially on a circuit board in a plating solution, wherein the pulse electroplating includes repeated forward pulses and reverse pulses performed sequentially;

[0066] The current density of DC plating was 15 ASF and the time was 30 min;

[0067] The current density of the forward pulse was 15 ASF, the pulse width was 40 ms, the current density of the reverse pulse was 50 ASF, the pulse width was 2 ms, and the pulse plating time was 30 min;

[0068] The distance between the cathode and the anode in the pattern electroplating process is 180 mm, and the temperature of the plating solution is 22°C;

[0069] The solutes of the plating solution include: copper sulfate pentahydrate with a concentration of 240 g / L, 98 wt% concentrated sulfuric acid with a concentration of 100 g / L and potassium chloride with a concentration of 45 ppm, and the solvent is water.

[0070] Example 4

[0071] This embodiment provides a pattern electroplating process, which includes a first stage of direct current electroplating, a first stage of pulse electroplating, a second stage of direct current electroplating and a second stage of pulse electroplating performed sequentially on a circuit board in a plating solution;

[0072] The first stage of DC plating:

[0073] The current density of DC plating was 8ASF and the time was 20min;

[0074] The first pulse plating:

[0075] The current density of the forward pulse is 22ASF, the pulse width is 25ms, the current density of the reverse pulse is 66ASF, the pulse width is 1ms, and the first pulse plating time is 40min;

[0076] The second stage of DC plating:

[0077] The current density of DC plating is 22ASF and the time is 20min;

[0078] The second pulse plating:

[0079] The current density of the forward pulse is 18ASF, the pulse width is 45ms, the current density of the reverse pulse is 10ASF, the pulse width is 1.8ms, and the second pulse plating time is 40min;

[0080] In the pattern electroplating process, the distance between the cathode and the anode is 250 mm, and the temperature of the plating solution is 24° C.;

[0081] The solutes of the plating solution include: copper sulfate pentahydrate with a concentration of 260 g / L, 98 wt % concentrated sulfuric acid with a concentration of 65 g / L, and sodium chloride with a concentration of 70 ppm, and the solvent is water.

[0082] Example 5

[0083] This embodiment provides a pattern electroplating process, which is the same as that of Embodiment 3 except that the pulse electroplating time is 15 minutes and the DC electroplating time is 45 minutes.

[0084] Example 6

[0085] This embodiment provides a pattern electroplating process, which is the same as that of Embodiment 3 except that the pulse electroplating time is 45 minutes and the DC electroplating time is 15 minutes.

[0086] Comparative Example 1

[0087] This comparative example provides a graphic electroplating process, which is the same as Example 1 except that the current density of the forward pulse is 10ASF and the current density of the reverse pulse is 40ASF.

[0088] Comparative Example 2

[0089] This comparative example provides a graphic electroplating process, which is the same as Example 1 except that the current density of the forward pulse is 20ASF and the current density of the reverse pulse is 5ASF.

[0090] Comparative Example 3

[0091] This comparative example provides a pattern electroplating process, which is the same as Example 1 except that the pulse width of the forward pulse is 15 ms and the pulse width of the reverse pulse is 1 ms.

[0092] Comparative Example 4

[0093] This comparative example provides a pattern electroplating process, wherein the pattern electroplating process is a circuit board subjected to a period of direct current electroplating in a plating solution, and the current density of the direct current electroplating is 20ASF;

[0094] The total time of the pattern electroplating process, i.e., the time of direct current electroplating, is 80 minutes;

[0095] In the pattern electroplating process, the distance between the cathode and the anode is 200 mm, and the temperature of the plating solution is 25°C;

[0096] The solutes of the plating solution include: copper sulfate pentahydrate with a concentration of 250 g / L, 98 wt% concentrated sulfuric acid with a concentration of 80 g / L, and sodium chloride with a concentration of 50 ppm, and the solvent is water.

[0097] An optical microscope was used to test the circuits with a line width of 25 μm after the pattern electroplating process in Example 1, Example 3, Example 4 and Comparative Example 4, respectively. The circuit diagram in Example 1 was obtained as shown in FIG. Figure 1 As shown, the circuit diagram in Example 3 is obtained as Figure 2 As shown, the circuit diagram in Example 4 is obtained as Figure 3 As shown, the circuit diagram in Comparative Example 4 is obtained as Figure 4 shown.

[0098] The lines with a line width of 25 μm obtained after the pattern electroplating process in Examples 1 to 6 and Comparative Examples 1 to 4 were measured using an optical microscope, and the average line height and arc rate of the lines were obtained as shown in Table 1;

[0099] Table 1

[0100]

[0101]

[0102] From Table 1, we can get:

[0103] (1) The arc rate of the circuit with a line width of 25 μm after the pattern electroplating process in Examples 1 to 4 is relatively low. The arc rate of the circuit obtained by the pattern electroplating process provided by the present invention is relatively low, reaching less than 17%, showing a rectangle that is more inclined to the ideal state;

[0104] (2) By comparing Example 3 with Examples 5 and 6, it can be seen that the ratio of the total time of pulse plating to the total time of DC plating in the graphic electroplating process will affect the size of the arc rate. When the ratio of the total time of pulse plating to the total time of DC plating is too small, the arc rate will become larger. This is because the proportion of the tip effect time of DC plating is large, and the curvature of the line becomes larger accordingly; when the ratio of the total time of pulse plating to the total time of DC plating is too large, the arc rate will become smaller. This is because the proportion of the tip effect time of DC plating is small, and the curvature of the line becomes smaller accordingly. However, the deposition speed of pulse plating is slow. If the ratio of the total time of pulse plating to the total time of DC plating is too large, the efficiency of the electroplating process will decrease.

[0105] (3) By comparing Example 1 with Comparative Examples 1 and 2, it can be seen that the ratio of the current density of the forward pulse to the current density of the reverse pulse in pulse electroplating will affect the size of the arc rate. When the ratio of the current density of the forward pulse to the current density of the reverse pulse is smaller, the arc rate will become smaller. This is because the positive and negative current ratio of the pulse is small, the proportion of the reverse current is large, and the effect of weakening the tip effect of the circuit is stronger. However, a smaller ratio of the current density of the forward pulse to the current density of the reverse pulse will lead to energy consumption, increased costs and reduced preparation efficiency; when the ratio of the current density of the forward pulse to the current density of the reverse pulse is larger, the arc rate will become larger. This is because the positive and negative current ratio of the pulse is large, the proportion of the reverse current is small, and the effect of weakening the tip effect of the circuit is weaker.

[0106] (4) By comparing Example 1 with Comparative Example 3, it can be seen that the ratio of the pulse width of the forward pulse to the pulse width of the reverse pulse in pulse electroplating will affect the size of the arc rate. When the ratio of the pulse width of the forward pulse to the pulse width of the reverse pulse is too small, the arc rate will become smaller. This is because the pulse width ratio of the positive and negative currents reflects the proportion of the operating time of the positive and negative currents. When the ratio of the pulse width of the forward pulse to the pulse width of the reverse pulse is too small, the proportion of the reverse current is too large, which weakens the tip effect of the circuit and reduces the arc rate. However, a small ratio of the pulse width of the forward pulse to the pulse width of the reverse pulse will lead to energy consumption, increased costs and reduced preparation efficiency.

[0107] (5) By comparing Example 1 with Comparative Example 4, it can be seen that the pattern electroplating process described in the present invention adopts pulse electroplating. Due to the existence of the tip effect during the forward pulse, the metal deposition speed on the circuit is faster; during the reverse pulse, the metal dissolves faster in the circuit. In the present invention, by limiting the ratio of the current density of the forward pulse to the current density of the reverse pulse and the ratio of the pulse width of the forward pulse to the pulse width of the reverse pulse, the problem of high arc rate of the circuit caused by the tip effect is eliminated.

[0108] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.

Claims

1. A pattern electroplating process, characterized in that: The pattern electroplating process includes performing at least one pulse electroplating of the circuit board in a plating solution, wherein each pulse electroplating includes a forward pulse and a reverse pulse that are repeated in sequence; The current density of the forward pulse is 10-25 ASF; the current density of the reverse pulse is 2.5-66 ASF; The ratio of the current density of the forward pulse to the current density of the reverse pulse is 1:(0.3-3); The ratio of the pulse width of the forward pulse to the pulse width of the reverse pulse is greater than or equal to 22:1; The pattern electroplating process further includes at least one section of direct current electroplating; the current density of each section of the direct current electroplating is 8-22 ASF; The pulse width of the forward pulse is 20-60 ms; the pulse width of the reverse pulse is 0.5-2 ms; The ratio of the total time of pulse plating to the total time of DC plating in the graphic electroplating process is 1:(0.5~2).

2. The pattern electroplating process according to claim 1, characterized in that: The total time of the pattern electroplating process is 50 to 120 minutes.

3. The pattern electroplating process according to claim 1, characterized in that: The distance between the cathode and the anode in the pattern electroplating process is 150-250 mm.

4. The pattern electroplating process according to claim 1, characterized in that: The temperature of the plating solution in the pattern electroplating process is 22-28°C.

5. The pattern electroplating process according to claim 1, characterized in that: The plating solution includes a copper plating solution.

6. The pattern electroplating process according to claim 5, characterized in that: The solute of the copper plating solution includes a copper source, concentrated sulfuric acid and a chlorine source.

7. The pattern electroplating process according to claim 6, characterized in that: The concentration of the copper source is 240-280 g / L.

8. The pattern electroplating process according to claim 6, characterized in that: The concentration of the concentrated sulfuric acid is 50-100 g / L.

9. The pattern electroplating process according to claim 6, characterized in that: The concentration of the chlorine source is 45-70 ppm.

10. The pattern electroplating process according to claim 1, characterized in that: The pattern electroplating process includes performing at least one section of direct current electroplating and at least one section of pulse electroplating on the circuit board in a plating solution; The current density of each section of direct current electroplating is 8-22 ASF; Each section of the pulse plating includes a forward pulse and a reverse pulse that are repeated in sequence, the current density of the forward pulse is 10-25 ASF, the pulse width of the forward pulse is 20-60 ms, the current density of the reverse pulse is 2.5-66 ASF, and the pulse width of the reverse pulse is 0.5-2 ms; The total time of the pattern electroplating process is 50-120 minutes, and the ratio of the total time of pulse electroplating to the total time of DC electroplating is 1:(0.5-2); In the pattern electroplating process, the distance between the cathode and the anode is 150-250 mm, and the temperature of the plating solution is 22-28° C.

11. A printed circuit board, characterized in that: The printed circuit board is obtained by the pattern electroplating process described in any one of claims 1 to 10, and the arc rate of the circuit of the printed circuit board is less than or equal to 17%.