Modified positive electrode particles for lithium battery and preparation method thereof, lithium battery positive electrode and all-solid-state lithium battery
By preparing a gradient electrolyte layer on the surface of the lithium battery cathode material, the problem of small contact area between electrolyte particles and cathode material and serious side reactions in all-solid-state lithium batteries is solved, and the battery performance and cathode material ratio are improved.
Patent Information
- Application Number
- CN202111063477.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-09-10
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2041-09-10
AI Technical Summary
In the existing all-solid-state lithium battery composite cathode layer, the contact area between the electrolyte particles and the cathode active material particles is small, the internal resistance is large, and the degree of side reactions is high, resulting in limited battery performance.
An electrolyte layer with gradient changes in ionic conductivity is prepared in situ on the surface of the cathode material. By adding Li2S and P2S5 solutions into the suspension in a protective atmosphere to react, an electrolyte layer with gradient changes is generated, wrapping the cathode material, and improving the interaction between the cathode material and the electrolyte. contact area and reduce interface reactions.
It improves the ionic conductivity of the cathode material, reduces the internal resistance and the degree of side reactions, improves battery performance, reduces the amount of electrolyte to a certain extent, and increases the proportion of active cathode materials.
Smart Images

Figure CN115799445B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium batteries, and in particular to modified positive electrode particles for lithium batteries and a preparation method thereof, a lithium battery positive electrode and an all-solid-state lithium battery. Background Art
[0002] As a low-carbon green new energy source, lithium-ion batteries have broad application prospects due to their high energy density, no memory effect and long cycle life. At present, the electrolytes in lithium-ion batteries mainly include organic liquid electrolytes and solid electrolytes; among them, solid electrolytes can greatly improve the safety performance of lithium batteries, so that they can be used in a wider range of fields.
[0003] In the existing all-solid-state battery composite positive electrode layer, such as Figure 1 As shown, the size of the electrolyte particles is relatively large, resulting in the correspondingly larger particles of the active positive electrode that match them, making the contact between the active positive electrode particles and the electrolyte particles a point contact between solids, resulting in a smaller contact area between the two, which hinders the transmission of ions and results in a higher internal resistance; secondly, the current electrolyte ion conductivity is relatively high, resulting in a high degree of side reactions with the positive electrode particles, which also leads to a higher interface impedance, seriously affecting the performance of the battery; in addition, larger electrolyte particles will also reduce the proportion of active positive electrodes in the positive electrode layer, which cannot reach the active positive electrode proportion of traditional liquid batteries, resulting in a lower surface capacity. Summary of the invention
[0004] The purpose of the present invention is to overcome the problems of small contact area between electrolyte particles and positive electrode active material particles, large internal resistance and high degree of side reactions in the composite positive electrode layer of an all-solid-state battery in the prior art, and to provide a lithium battery positive electrode material and a preparation method thereof, a lithium battery positive electrode and an all-solid-state lithium battery.
[0005] In order to achieve the above-mentioned object, the first aspect of the present invention provides a modified positive electrode particle for a lithium battery, wherein the modified positive electrode particle comprises a positive electrode material and an electrolyte layer wrapped on the surface of the positive electrode material; wherein the ionic conductivity of the electrolyte layer increases gradually from the positive electrode side of the electrolyte layer to the positive electrode side far away, and the ionic conductivity of the positive electrode side of the electrolyte layer is 10 -6 -10 -4 S / cm 2 The ionic conductivity of the electrolyte layer far from the positive electrode is 10 -3 -10 -2 S / cm 2 .
[0006] A second aspect of the present invention provides a method for preparing modified positive electrode particles for a lithium battery, the method comprising:
[0007] In a protective gas atmosphere, adding a Li2S solution and a P2S5 solution to a suspension containing a positive electrode material, reacting for 1.5-3 hours, to obtain the modified positive electrode particles;
[0008] wherein, per unit time, the molar ratio of Li2S to P2S5 added to the suspension gradually increases from 1-2:1 to 2.8-3.2:1; or
[0009] In unit time, the molar ratio of Li2S to P2S5 added to the suspension gradually decreases from 6-9:1 to 2.8-3.2:1.
[0010] The third aspect of the present invention provides a modified positive electrode particle for a lithium battery prepared according to the method described in the second aspect.
[0011] The fourth aspect of the present invention provides a lithium battery positive electrode, including a positive electrode collector and a positive electrode material layer coated on the surface of the positive electrode collector, wherein the positive electrode material layer contains a conductive agent, a first adhesive, and the modified positive electrode particles for lithium batteries described in the first aspect or the third aspect.
[0012] A fifth aspect of the present invention provides an all-solid-state lithium battery, comprising a positive electrode, a negative electrode and a solid electrolyte layer, wherein the positive electrode is the positive electrode of the lithium battery described in the fourth aspect.
[0013] Through the above technical scheme, the present invention prepares a uniform electrolyte layer with a gradient ion conductivity in situ on the surface of the positive electrode material, so that the electrolyte uniformly wraps the positive electrode material, increases the contact area between the positive electrode material and the electrolyte, and reduces the internal resistance of the positive electrode active material; secondly, the ion conductivity of the electrolyte layer changes in a gradient, the ion conductivity near the positive electrode side is lower, which can reduce the degree of side reactions at the interface; while the ion conductivity far from the positive electrode side is higher, which can construct an ion conduction network of the positive electrode layer and improve the ion conductivity of the positive electrode; it can greatly reduce the amount of electrolyte used, increase the proportion of active positive electrode materials, and reduce the occurrence of side reactions, thereby improving the performance of the positive electrode. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 It is a schematic diagram of the contact between electrolyte particles and active positive electrode particles in the prior art;
[0015] Figure 2 Schematic diagram of the structure of modified positive electrode particles according to one embodiment of the present invention.
[0016] Description of Reference Numerals
[0017] 1. Cathode material 2. Electrolyte layer DETAILED DESCRIPTION
[0018] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0019] As mentioned above, the first aspect of the present invention provides a modified positive electrode particle for a lithium battery, wherein the modified positive electrode particle comprises a positive electrode material and an electrolyte layer wrapped on the surface of the positive electrode material; wherein the ionic conductivity of the electrolyte layer increases gradually from the positive electrode side of the electrolyte layer to the positive electrode side, and the ionic conductivity of the positive electrode side of the electrolyte layer is 10 -6 -10 -4 S / cm 2 The ionic conductivity of the electrolyte layer far from the positive electrode is 10 -3 -10 -2 S / cm 2 ; The electrolyte layer comprises a first solid electrolyte.
[0020] Figure 2 is a schematic diagram of the structure of a modified positive electrode particle according to an embodiment of the present invention, such as Figure 2 As shown, the cathode-proximal side of the electrolyte layer refers to the side of the electrolyte layer adjacent to the cathode material; the cathode-distal side refers to the side of the electrolyte layer away from the cathode material.
[0021] In the present invention, the surface of the modified positive electrode particles provided by the present invention is coated with an electrolyte layer with a gradient ion conductivity, which can not only increase the contact area between the positive electrode material and the electrolyte, but also reduce the internal resistance of the positive electrode active material; secondly, the ion conductivity of the electrolyte layer changes in a gradient, the ion conductivity near the positive electrode side is lower, which can reduce the degree of side reactions at the interface; while the ion conductivity far from the positive electrode side is higher, which can construct an ion conduction network of the positive electrode layer and improve the ion conductivity of the positive electrode; and can greatly reduce the amount of electrolyte used, increase the proportion of active positive electrode materials, and at the same time reduce the occurrence of side reactions, thereby improving the performance of the positive electrode.
[0022] In some preferred embodiments of the present invention, the thickness of the electrolyte layer is 1-6 μm, preferably 2-4 μm; further preferably, based on the total amount of the modified positive electrode particles, the content of the electrolyte layer is 5-30 wt%, and the content of the positive electrode material is 70-95 wt%. Under the above preferred conditions, the amount of the first solid electrolyte in the modified positive electrode particles can be reduced and the content of the positive electrode material can be increased while reducing the side reaction of the positive electrode material and ensuring the electrical properties of the positive electrode material.
[0023] According to the present invention, under preferred conditions, the electrolyte layer comprises a sulfur-based solid electrolyte and a non-electrolyte material, wherein the non-electrolyte material is selected from Li2S and / or P2S5; further preferably, the sulfur-based solid electrolyte is selected from Li x M y P z S w , doped Li x M y P z S w and Li a P b S c Cl d At least one of the following, wherein M is selected from at least one of Si, Ge and Sn, and x+4y+5z=2w, 0≤y≤1.5, a+5b=2c+d; x, z, w, a, b, c, d are all greater than zero.
[0024] In the present invention, y may be zero or non-zero; more preferably, when y≠0, Li x M y P z S w It can be Li 10 GeP2S 12 , LiSnPS, LiAsPS, LiSiPS; when y = 0, Li x P z S w (LPS) can be Li7P3S 11 and / or Li3PS4, among which Li7P3S 11 It can be crystalline Li7P3S 11 It can also be glassy Li7P3S 11 .
[0025] According to the present invention, under preferred conditions, the electrolyte layer is a mixture of Li3PS4 and Li2S or a mixture of Li3PS4 and P2S5.
[0026] When the sulfur-based solid electrolyte is a mixture of Li3PS4 and Li2S, the molar ratio of phosphorus to sulfur in the electrolyte layer gradually increases from 1:5-7 on the side near the positive electrode to 1:3.8-4.2 on the side far from the positive electrode; under the above preferred conditions, the content of Li3PS4 gradually increases from 33 mol% on the side near the positive electrode to 100 mol% on the side far from the positive electrode, and the content of Li2S gradually decreases from 67 mol% on the side near the positive electrode to 0 on the side far from the positive electrode, so that the ionic conductivity of the electrolyte layer gradually increases from the side near the positive electrode to the side far from the positive electrode.
[0027] When the electrolyte layer is a mixture of Li3PS4 and P2S5, the molar ratio of phosphorus to sulfur in the electrolyte layer gradually increases from 1:3-3.5 on the side near the positive electrode to 1:3.8-4.2 on the side far from the positive electrode; under the above preferred conditions, the content of Li3PS4 gradually increases from 66 mol% on the side near the positive electrode to 100 mol% on the side far from the positive electrode, and the content of P2S5 gradually decreases from 33 mol% on the side near the positive electrode to 0 on the side far from the positive electrode; so that the ionic conductivity of the electrolyte layer gradually increases from the side near the positive electrode to the side far from the positive electrode.
[0028] In some preferred embodiments of the present invention, the positive electrode material is a coated or uncoated Li(Ni m Co n Mn 1-m-n )O2, wherein 0≤m≤1, 0≤n≤1, and m+n≤1, for example, it can be at least one of LiCoO2, LiMnO2, and LiNiO2; when the positive electrode material is coated Li(Ni m Co n Mn 1-m-n )O2, coated on the Li(Ni m Co n Mn 1-m-n )The coating layer on the surface of O2 is selected from at least one of lithium niobate, lithium titanate, lithium zirconate and lithium phosphate.
[0029] According to the present invention, under preferred conditions, the particle size D50 of the positive electrode material is 3-15 μm.
[0030] A second aspect of the present invention provides a method for preparing modified positive electrode particles for a lithium battery, the method comprising:
[0031] In a protective gas atmosphere, the Li2S solution and the P2S5 solution are simultaneously added to the suspension containing the positive electrode material, and reacted for 1.5-3 hours to obtain the modified positive electrode particles;
[0032] wherein, per unit time, the molar ratio of Li2S to P2S5 added to the suspension gradually increases from 1-2:1 to 2.8-3.2:1; or
[0033] In unit time, the molar ratio of Li2S to P2S5 added to the suspension gradually decreases from 6-9:1 to 2.8-3.2:1.
[0034] In the present invention, when the Li2S solution and the P2S5 solution are added to the suspension at the same time, P2S5 and Li2S can react on the surface of the positive electrode material to generate Li3PS4, and the chemical reaction formula is 3Li2S+P2S5=2Li3PS4; when Li2S is in excess, the reaction formula becomes (3+p)Li2S+P2S5=2Li3PS4+pLi2S, and the reaction product is a mixed phase of LPS (Li3PS4) and Li2S; conversely, when P2S5 is in excess, the reaction formula becomes 3Li2S+(1+q)P2S5=2Li3PS4+q P2S5, and the reactant is a mixture of Li3PS4 and P2S5. The present invention controls the dropping rates of the Li2S solution and the P2S5 solution and the molar ratio of Li2S to P2S5 in the reaction system, thereby in-situ generating an electrolyte layer with gradient components on the surface of the positive electrode material, and controlling the content of each component in the generated electrolyte layer and the ionic conductivity of the electrolyte layer.
[0035] According to the present invention, the method further comprises: vacuum drying the modified positive electrode particles, and the vacuum drying method may be known to those skilled in the art; illustratively, the vacuum drying temperature may be 60-100° C., and the time may be 12-48 hours.
[0036] In the present invention, under preferred conditions, the method further comprises: dispersing the positive electrode material in a first organic solvent to obtain a suspension of the positive electrode material. Preferably, in the suspension, the mass concentration of the positive electrode material is 100-300 g / L, preferably 150-250 g / L.
[0037] Further preferably, the method further comprises: dissolving Li2S in a second organic solvent to obtain a Li2S solution; preferably, the mass concentration of the Li2S solution is 4-6wt%.
[0038] Further preferably, the method further comprises: dissolving P2S5 in a third organic solvent to obtain a P2S5 solution; preferably, the mass concentration of P2S5 in the P2S5 solution is 20-25wt%.
[0039] According to the present invention, the first organic solvent, the second organic solvent and the third organic solvent are all solvents that are stable to electrolytes; under preferred conditions, the first organic solvent, the second organic solvent and the third organic solvent are each independently selected from at least one of toluene, xylene, trimethylbenzene, acetonitrile, tetrahydrofuran, anisole, n-heptane and n-decane. In the present invention, the first organic solvent, the second organic solvent and the third organic solvent may be the same or different, preferably the first organic solvent, the second organic solvent and the third organic solvent are the same; most preferably, the first organic solvent, the second organic solvent and the third organic solvent are all acetonitrile.
[0040] According to the present invention, in the above method, the positive electrode material is a coated or uncoated Li(Ni m Co n Mn 1-m-n )O2, wherein 0≤m≤1, 0≤n≤1, and m+n≤1, for example, it can be at least one of LiCoO2, LiMnO2, and LiNiO2; when the positive electrode material is coated Li(Ni m Co n Mn 1-m-n )O2, coated on the Li(Ni m Co n Mn 1-m-n )The coating layer on the surface of O2 is selected from at least one of lithium niobate, lithium titanate, lithium zirconate and lithium phosphate; preferably, the particle size D50 of the positive electrode material is 3-15μm.
[0041] The present invention can increase the contact area between the positive electrode material and the solid electrolyte by wrapping the electrolyte layer on the surface of the positive electrode material, and no additional electrolyte needs to be added during the subsequent electrode preparation process.
[0042] The third aspect of the present invention provides a modified positive electrode particle for a lithium battery prepared by the method described in the second aspect; the modified positive electrode particle comprises a positive electrode material and an electrolyte layer wrapped on the surface of the positive electrode material; wherein the ionic conductivity of the electrolyte layer increases gradually from the positive electrode side to the far positive electrode side of the electrolyte layer, and the ionic conductivity of the positive electrode side of the electrolyte layer is 10 -5 -10 -4 S / cm 2 The ionic conductivity of the electrolyte layer far from the positive electrode is 10 -3 -10 -2 S / cm 2 .
[0043] The fourth aspect of the present invention provides a lithium battery positive electrode, including a positive electrode collector and a positive electrode material layer coated on the surface of the positive electrode collector, wherein the positive electrode material layer contains a conductive agent, a first adhesive, and the modified positive electrode particles for lithium batteries described in the first aspect or the third aspect.
[0044] According to the present invention, preferably, the conductive agent is selected from at least one of graphite, acetylene black, graphene, and carbon black; further preferably, the first adhesive is a fluorine-containing resin and / or a polyolefin compound, preferably at least one of polyvinylidene fluoride, polytetrafluoroethylene, nitrile rubber, and styrene-butadiene rubber.
[0045] In a preferred embodiment of the present invention, based on the total mass of the positive electrode material layer, the positive electrode material layer comprises 1-10 wt % of a conductive agent, 1-10 wt % of a binder and 80-98 wt % of modified positive electrode particles.
[0046] A fifth aspect of the present invention provides an all-solid-state lithium battery, comprising a positive electrode, a negative electrode and a solid electrolyte layer, wherein the positive electrode is the positive electrode of the lithium battery described in the fourth aspect.
[0047] In some preferred embodiments of the present invention, the solid electrolyte layer consists of a solid electrolyte and a second binder.
[0048] In some preferred embodiments of the present invention, the solid electrolyte is selected from Li x M y P z S w and / or doped Li x M y P z S w , wherein M is selected from one or more of Si, Ge and Sn, x+4y+5z=2w, 0≤y≤1.5, x>0, z>0, w>0; preferably 0<y≤1.5; further preferably, the second solid electrolyte is Li 10 GeP2S 12 , at least one of LiSnPS, LiAsPS and LiSiPS.
[0049] According to the present invention, under preferred conditions, the second binder is selected from at least one of polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polystyrene, polybutadiene, acrylic resin, epoxy resin, polyethylene oxide, sodium carboxymethyl cellulose and styrene-butadiene latex.
[0050] Further preferably, based on the total mass of the solid electrolyte layer, the solid electrolyte layer comprises 0.1-10 wt % of the second binder and 90-99.9 wt % of the solid electrolyte.
[0051] In the present invention, the negative electrode includes a negative electrode current collector and a negative electrode material layer coated on the surface of the negative electrode current collector, wherein the negative electrode material layer contains a negative electrode active material and a third binder, wherein the type of the negative electrode active material can be known to those skilled in the art, preferably a negative electrode active material that can deintercalate lithium, for example, it can be at least one of a carbon material, metallic lithium, a lithium-indium alloy and silicon, and the carbon material is preferably at least one of graphite, acetylene black, graphene and activated carbon. The type of the third binder can be known to those skilled in the art, for example, it can be at least one of polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polystyrene, polybutadiene, acrylic resin, epoxy resin, polyethylene oxide, sodium carboxymethyl cellulose and styrene-butadiene latex; preferably, based on the total amount of the negative electrode material layer, the negative electrode material layer contains 0.1-10wt% of the third binder and 90-99.9wt% of the negative electrode active material.
[0052] In the present invention, the preparation method of the all-solid-state lithium battery may be known to those skilled in the art. Exemplarily, the preparation method of the all-solid-state lithium battery includes:
[0053] (1) mixing a first binder in an organic solvent to form a uniform binder solution; then uniformly dispersing the modified positive electrode particles and the conductive agent in the binder solution, and fully stirring and mixing to obtain a composite positive electrode slurry; then coating the composite positive electrode slurry on a current collector, and then drying and rolling to obtain a lithium battery positive electrode;
[0054] (2) uniformly dispersing a second solid electrolyte and a second adhesive in an organic solvent to form a slurry; then coating the slurry on the positive electrode of the lithium battery, followed by drying and rolling to obtain a composite layer of a solid electrolyte layer and a positive electrode of the lithium battery;
[0055] (3) uniformly dispersing the third binder and the negative electrode active material in an organic solvent to form a negative electrode slurry; then coating the negative electrode slurry on a negative electrode current collector, and then drying and rolling to obtain a negative electrode for a lithium battery;
[0056] (4) After the composite layer of the solid electrolyte layer and the lithium battery positive electrode and the lithium battery negative electrode are stacked, they are pressed by a roller press, wherein the pressing pressure is 0.5-10 MPa.
[0057] The present invention will be described in detail below through examples.
[0058] In the following examples, lithium cobalt oxide is a commercially available product of Tianjin Bamo BM4500, and its particle size (D50) is 6 μm.
[0059] In the following examples, the thickness of the electrolyte layer was measured by a high-resolution scanning electron microscope (SEM) method; and the molar ratio of phosphorus atoms to sulfur atoms in the near-electrode side of the electrolyte layer and the far-electrode side of the electrolyte layer was tested by EDS.
[0060] Ion conductivity test: Based on the molar ratio of phosphorus atoms to sulfur atoms in the electrolyte layer obtained by EDS test, an electrolyte with the same composition is synthesized, and then the electrochemical impedance spectroscopy (EIS) of the electrolyte is measured by an electrochemical workstation to calculate the conductivity of the electrolyte.
[0061] In the following examples, the preparation method of suspension A is as follows: in a nitrogen atmosphere, 100 g of lithium cobalt oxide and 500 mL of acetonitrile are mixed uniformly to form suspension A (suspension of positive electrode material);
[0062] Preparation method of solution B: In a nitrogen atmosphere, 5 g of Li2S and 121 mL of acetonitrile were mixed evenly to form solution B (5 wt% Li2S acetonitrile solution);
[0063] Preparation method of solution C: In a nitrogen atmosphere, 23 g of P2S5 and 98 mL of acetonitrile were mixed evenly to form solution C (23 wt % P2S5 acetonitrile solution).
[0064] Example 1
[0065] (1) In situ synthesis of modified cathode particles
[0066] In this embodiment, in the initial synthesis stage, the content of P2S5 in the system is excessive, and the ratio of Li2S to P2S5 in the system is gradually increased by gradually increasing the drop rate of solution B, as follows:
[0067] In a nitrogen atmosphere, solution B was added to suspension A at a drop rate of 0.07 g / min, and solution C was added to the suspension A at a drop rate of 0.07 g / min, and the reaction was stirred and reacted for 10 min while maintaining the drop rate;
[0068] Then, the dropping rate of solution B was adjusted to 0.13 g / min, and the stirring reaction was maintained at this dropping rate for 20 min;
[0069] Then, the dropping rate of solution B was adjusted to 0.2 g / min, and the dropping rate was maintained for stirring and reacting for 90 min to obtain a mixed system;
[0070] The residue obtained by filtering the mixed system was vacuum dried at 80° C. for 24 h, and then ground to obtain modified positive electrode particles;
[0071] The physical properties of the modified positive electrode particles are shown in Table 1.
[0072] (2) Preparation of composite positive electrode layer
[0073] In a nitrogen environment of a glove box, 15 g of a binder SBR and 500 mL of xylene were stirred and mixed to obtain a binder solution; 200 g of modified positive electrode particles and 10 g of a conductive agent SuperP were placed in the above-mentioned binder solution and stirred to form a uniformly dispersed composite positive electrode slurry. The composite positive electrode slurry was evenly coated on an aluminum foil (aluminum foil size: width 160 mm, thickness 16 μm) using a coating machine, and then dried and rolled to obtain a lithium battery positive electrode.
[0074] (3) Fabrication of solid electrolyte layer
[0075] In a glove box with nitrogen atmosphere, 500 g Li 10 GeP2S 12 20 g of polyvinylidene fluoride (PVDF) and 1000 mL of toluene are mixed evenly to obtain a slurry, and then a coating machine is used to evenly coat the slurry on the lithium battery positive electrode in step (2), and then dried, rolled, and cut to obtain a composite layer of a lithium battery positive electrode + solid electrolyte layer with a size of 50 mm × 200 mm.
[0076] (4) Preparation of negative electrode
[0077] 500g of negative electrode active material graphite, 20g of thickener sodium carboxymethyl cellulose (CMC), and 10g of styrene-butadiene rubber (SBR) were mixed evenly in 1000mL of deionized water to obtain a negative electrode slurry; then a coating machine was used to evenly coat the negative electrode slurry on a copper foil (copper foil size: 160mm wide and 16mm thick), and then dried, pressed, and cut to obtain a negative electrode with a size of 50mm×200mm.
[0078] (5) Assembly of all-solid-state lithium batteries
[0079] In the inert atmosphere of the glove box, align the lithium battery positive electrode + solid electrolyte layer obtained in step (3) and the negative electrode prepared in step (4), press them together using a roller press (the roller pressure is 3 MPa, and the roller speed is 1 rpm), and then cut them into discs with a diameter of 15 mm using a cutting machine, and encapsulate them in a button battery shell to obtain an all-solid-state lithium battery.
[0080] Example 2
[0081] In this embodiment, in the initial synthesis stage, the content of Li2S in the system is excessive, and the ratio of Li2S to P2S5 in the system is gradually reduced by gradually reducing the drop rate of solution B, as follows:
[0082] According to the method of Example 1, the difference is that the preparation method of the modified positive electrode particles is as follows:
[0083] (1) In situ synthesis of modified cathode particles
[0084] In a nitrogen atmosphere, solution B was added to suspension A at a drop rate of 0.4 g / min, and solution C was added to the suspension A at a drop rate of 0.07 g / min, and the reaction was stirred and reacted for 10 min while maintaining the drop rate;
[0085] Then, the dropping rate of solution B was adjusted to 0.3 g / min, and the stirring reaction was maintained at this dropping rate for 20 min;
[0086] Then, the dropping rate of solution B was adjusted to 0.2 g / min, and the dropping rate was maintained for stirring and reacting for 90 min to obtain a mixed system;
[0087] The filter residue obtained by filtering the mixed system was vacuum dried at 80° C. for 24 h, and then ground to obtain modified positive electrode particles; the physical properties of the modified positive electrode particles are shown in Table 1.
[0088] The preparation of the composite positive electrode layer, the solid electrolyte layer, the negative electrode and the assembly of the all-solid-state lithium battery are the same as in Example 1 to obtain a lithium battery A2.
[0089] Example 3
[0090] According to the method of Example 1, in the initial synthesis stage, the content of P2S5 in the system is excessive, except that the dripping rate of solution B is different from that of Example 1. The preparation method of the modified positive electrode particles is as follows:
[0091] (1) In situ synthesis of modified cathode particles
[0092] In a nitrogen atmosphere, solution B was added to suspension A at a drop rate of 0.14 g / min, and solution C was added to the suspension A at a drop rate of 0.07 g / min, and the reaction was stirred and reacted for 10 min while maintaining the drop rate;
[0093] Then, the dropping rate of solution B was adjusted to 0.2 g / min, and the dropping rate of solution C was kept unchanged, and the stirring reaction was maintained at this dropping rate for 110 min to obtain a mixed system;
[0094] The filter residue obtained by filtering the mixed system was vacuum dried at 80° C. for 24 h, and then ground to obtain modified positive electrode particles; the physical properties of the modified positive electrode particles are shown in Table 1.
[0095] The preparation of the composite positive electrode layer, the solid electrolyte layer, the negative electrode and the assembly of the all-solid-state lithium battery are the same as in Example 1 to obtain a lithium battery A3.
[0096] Example 4
[0097] According to the method of Example 2, in the initial synthesis stage, the content of Li2S in the system is excessive, and the ratio of Li2S to P2S5 in the system is gradually reduced by gradually increasing the dripping rate of solution C, as follows:
[0098] (1) In situ synthesis of modified cathode particles
[0099] In a nitrogen atmosphere, solution B was added to suspension A at a drop rate of 0.6 g / min, and solution C was added to the suspension A at a drop rate of 0.07 g / min, and the reaction was stirred and reacted for 10 min while maintaining the drop rate;
[0100] Then, the dropping rate of solution C was adjusted to 0.14 g / min, and the dropping rate of solution B was kept unchanged, and the stirring reaction was maintained at this dropping rate for 20 min;
[0101] Then, the dropping rate of solution C was adjusted to 0.2 g / min, and the dropping rate of solution B was kept unchanged, and the stirring reaction was maintained at this dropping rate for 90 min to obtain a mixed system;
[0102] The filter residue obtained by filtering the mixed system was vacuum dried at 80° C. for 24 h, and then ground to obtain modified positive electrode particles; the physical properties of the modified positive electrode particles are shown in Table 1.
[0103] The preparation of the composite positive electrode layer, the solid electrolyte layer, the negative electrode and the assembly of the all-solid-state lithium battery were the same as in Example 1 to obtain a lithium battery A4.
[0104] Example 5
[0105] According to the method of Example 1, in the initial synthesis stage, the content of P2S5 in the system is excessive, except that: by gradually reducing the dripping rate of solution C, the ratio of Li2S to P2S5 in the system is gradually increased, and the preparation method of the modified positive electrode particles is as follows:
[0106] (1) In situ synthesis of modified cathode particles
[0107] In a nitrogen atmosphere, solution B was added to suspension A at a drop rate of 0.6 g / min, and solution C was added to the suspension A at a drop rate of 0.4 g / min, and the reaction was stirred and reacted for 10 min while maintaining the drop rate;
[0108] Then, the dropping rate of solution C was adjusted to 0.3 g / min, and the dropping rate of solution B was kept unchanged, and the stirring reaction was maintained at this dropping rate for 20 min;
[0109] Then, the dropping rate of solution C was adjusted to 0.2 g / min, and the dropping rate of solution B was kept unchanged, and the stirring reaction was maintained at this dropping rate for 90 min to obtain a mixed system;
[0110] The filter residue obtained by filtering the mixed system was vacuum dried at 80° C. for 24 h, and then ground to obtain modified positive electrode particles; the physical properties of the modified positive electrode particles are shown in Table 1.
[0111] The preparation of the composite positive electrode layer, the solid electrolyte layer, the negative electrode and the assembly of the all-solid-state lithium battery are the same as in Example 1 to obtain a lithium battery A5.
[0112] Example 6
[0113] According to the method of Example 1, the difference is that the preparation method of the modified positive electrode particles is as follows:
[0114] (1) In situ synthesis of modified cathode particles
[0115] In a nitrogen atmosphere, solution B was added to suspension A at a drop rate of 0.07 g / min, and solution C was added to the suspension A at a drop rate of 0.07 g / min, and the reaction was stirred and reacted for 5 min while maintaining the drop rate;
[0116] Then, the dropping rate of solution B was increased to 0.14 g / min, and the dropping rate of solution C was kept unchanged, and the stirring reaction was maintained at this dropping rate for 10 min;
[0117] Then, the dropping rate of solution B was increased to 0.2 g / min, and the dropping rate of solution C was kept unchanged, and the stirring reaction was maintained at this dropping rate for 45 min to obtain a mixed system;
[0118] The filter residue obtained by filtering the mixed system was vacuum dried at 80° C. for 24 h, and then ground to obtain modified positive electrode particles; the physical properties of the modified positive electrode particles are shown in Table 1.
[0119] The preparation of the composite positive electrode layer, the solid electrolyte layer, the negative electrode and the assembly of the all-solid-state lithium battery are the same as in Example 1 to obtain a lithium battery A6.
[0120] Example 7
[0121] According to the method of Example 1, the difference is that the preparation method of the modified positive electrode particles is as follows:
[0122] (1) In situ synthesis of modified cathode particles
[0123] In a nitrogen atmosphere, solution B was added to suspension A at a drop rate of 0.07 g / min, and solution C was added to the suspension A at a drop rate of 0.07 g / min, and the reaction was stirred and reacted for 15 min while maintaining the drop rate;
[0124] Then, the dropping rate of solution B was increased to 0.14 g / min, and the dropping rate of solution C was kept unchanged, and the stirring reaction was maintained at this dropping rate for 30 min;
[0125] Then, the dropping rate of solution B was increased to 0.2 g / min, and the dropping rate of solution C was kept unchanged, and the stirring reaction was maintained at this dropping rate for 105 min to obtain a mixed system;
[0126] The filter residue obtained by filtering the mixed system was vacuum dried at 80° C. for 24 h, and then ground to obtain modified positive electrode particles; the physical properties of the modified positive electrode particles are shown in Table 1.
[0127] The preparation of the composite positive electrode layer, the production of the solid electrolyte layer, the production of the negative electrode and the assembly of the all-solid-state lithium battery are the same as in Example 1, to obtain a lithium battery A7.
[0128] Comparative Example 1
[0129] According to the method of Example 1, the difference is that the preparation method of the modified positive electrode particles is as follows:
[0130] (1) In situ synthesis of modified cathode particles
[0131] In a nitrogen atmosphere, solution B was added to suspension A at a dropping rate of 0.2 g / min, and solution C was added to the suspension A at a dropping rate of 0.2 g / min, and the dropping rate was maintained for stirring and reacting for 120 min to obtain a mixed system;
[0132] The filter residue obtained by filtering the mixed system was vacuum dried at 80° C. for 24 h, and then ground to obtain modified positive electrode particles; the physical properties of the modified positive electrode particles are shown in Table 1.
[0133] The preparation of the composite positive electrode layer, the solid electrolyte layer, the negative electrode and the assembly of the all-solid-state lithium battery were the same as in Example 1 to obtain a lithium battery B1.
[0134] Comparative Example 2
[0135] According to the method of Example 1, the difference is that lithium cobalt oxide is directly mixed with the electrolyte, wherein the preparation method of the electrolyte is as follows:
[0136] The solution B and the solution C are mixed and stirred for 120 minutes to obtain a mixed system; the residue obtained by filtering the mixed system is vacuum dried at 80° C. for 24 hours, and then ground to obtain solid electrolyte particles;
[0137] The preparation method of the positive electrode is as follows:
[0138] In a nitrogen environment of a glove box, 15 g of a binder SBR and 500 mL of xylene were stirred and mixed to obtain a binder solution; 200 g of lithium cobalt oxide, 100 g of solid electrolyte particles and 10 g of a conductive agent SuperP were placed in the above-mentioned binder solution and stirred to form a uniformly dispersed composite positive electrode slurry. The composite positive electrode slurry was evenly coated on an aluminum foil (aluminum foil size: width 160 mm, thickness 16 um) using a coating machine, and then dried and rolled to obtain a lithium battery positive electrode.
[0139] Table 1
[0140]
[0141] In Table 1, the near positive electrode side refers to the side of the electrolyte layer close to the positive electrode material; the far positive electrode side refers to the side of the electrolyte layer away from the positive electrode material; the middle refers to the half of the thickness of the electrolyte layer.
[0142] It can be seen from Table 1 that the composition of the electrolyte layer of the modified positive electrode particles of the present invention changes in a gradient, and the ionic conductivity of the electrolyte layer also gradually increases from the positive electrode side to the positive electrode side.
[0143] 2. Electrical performance test
[0144] The all-solid-state lithium batteries obtained in Examples 1-7 and Comparative Examples 1-2 were subjected to charge and discharge cycle tests, the test contents including initial specific capacity (mAh / g) and cycle life, and the test method was as follows:
[0145] (1) The test equipment is LAND CT 2001C secondary battery performance test device, the test temperature is room temperature (25°C), and the all-solid-state lithium battery is subjected to a charge and discharge cycle test at 0.1C. The test procedure steps are set as follows: stand for 10 minutes; charge at constant voltage to 4.3V cutoff; stand for 10 minutes; discharge at constant current to 3V, which is 1 cycle. Repeat this step, and set the capacity remaining at the current cycle number to 80% of the initial capacity, which is the cycle life of the battery.
[0146] The calculation method of the positive electrode material ratio is as follows:
[0147] Positive electrode material ratio = positive electrode material mass ÷ total mass of composite positive electrode layer × 100%;
[0148] Among them, the total mass of the composite positive electrode layer refers to the total mass of the positive electrode material, the electrolyte layer, the conductive agent and the binder. In the above embodiments and comparative examples, the positive electrode material refers to lithium cobalt oxide; the electrolyte layer refers to the mass of the electrolyte layer wrapped on the surface of the lithium cobalt oxide.
[0149] Table 2
[0150]
[0151] It can be seen from the results in Table 2 that in the embodiment of the present invention, the content of the positive electrode particles is as high as 82wt%, and the specific capacity and cycle life of the obtained all-solid-state battery are higher than those of Comparative Example 1 (no gradient change in the electrolyte) and Comparative Example 2 (non-in-situ synthesis of the positive electrode layer); In Example 7, due to the large thickness of the electrolyte layer, the proportion of the positive electrode material in the composite positive electrode layer is low, but because the electrolyte layer is conducive to increasing the ion path, the specific capacity of the lithium battery is relatively high.
[0152] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A modified positive electrode particle for a lithium battery, It is characterized in that The modified positive electrode particles include a positive electrode material and an electrolyte layer wrapped on the surface of the positive electrode material; wherein the ionic conductivity of the electrolyte layer increases gradually from the positive electrode side to the far positive electrode side of the electrolyte layer, and the ionic conductivity of the positive electrode side of the electrolyte layer is 10 -6 -10 -4 S / cm 2 The ionic conductivity of the electrolyte layer far from the positive electrode is 10 -3 -10 -2 S / cm 2 .
2. The modified positive electrode particle according to claim 1, in, The thickness of the electrolyte layer is 1-6 μm.
3. The modified positive electrode particle according to claim 2, in, Based on the total amount of the modified positive electrode particles, the content of the electrolyte layer is 5-30wt%, and the content of the positive electrode material is 70-95wt%.
4. The modified positive electrode particle according to claim 1, in, The electrolyte layer comprises a sulfur-based solid electrolyte and a non-electrolyte material, wherein the non-electrolyte material is selected from Li 2 S and / or P 2 S 5 .
5. The modified positive electrode particle according to claim 4, in, The sulfur-based solid electrolyte is selected from Li x M y P z S w , doped Li x M y P z S w and Li a P b S c Cl d At least one of the following, wherein M is selected from at least one of Si, Ge and Sn, and x+4y+5z=2w, 0≤y≤1.5, a+5b=2c+d; x, z, w, a, b, c, d are all greater than zero.
6. The modified positive electrode particle according to claim 5, in, The Li x M y P z S w For Li 7 P 3 S 11 and / or Li 3 PS 4 .
7. The modified positive electrode particle according to any one of claims 4 to 6, in, The electrolyte layer is selected from Li 3 PS 4 With Li 2 A mixture of S or Li 3 PS 4 With P 2 S 5 mixture.
8. The modified positive electrode particle according to claim 4, in, When the electrolyte layer is Li 3 PS 4 With Li 2 When the mixture is composed of sulfur and phosphorus, the molar ratio of phosphorus to sulfur in the electrolyte layer gradually increases from 1:5-7 on the side close to the positive electrode to 1:3.8-4.2 on the side far from the positive electrode.
9. The modified positive electrode particle according to claim 8, in, When the electrolyte layer is Li 3 PS 4 With P 2 S 5 When a mixture of phosphorus and sulfur is prepared, the molar ratio of phosphorus to sulfur in the electrolyte layer gradually increases from 1:3-3.5 on the side close to the positive electrode to 1:3.8-4.2 on the side far from the positive electrode.
10. The modified positive electrode particle according to claim 1, in, The positive electrode material is coated or uncoated Li(Ni m Co n Mn 1-m-n ) 2 , where 0≤m≤1, 0≤n≤1, and m+n≤1.
11. The modified positive electrode particle according to claim 10, in, When the positive electrode material is coated Li(Ni m Co n Mn 1-m-n ) 2 When coated on the Li(Ni m Co n Mn 1-m-n ) 2 The surface coating layer is selected from at least one of lithium niobate, lithium titanate, lithium zirconate and lithium phosphate.
12. The modified positive electrode particle according to claim 10 or 11, in, The particle size D50 of the positive electrode material is 3-15 μm.
13. A method for preparing modified positive electrode particles for lithium batteries, It is characterized in that The method comprises: In a protective gas atmosphere, Li 2 S solution and P 2 S 5 The solution is simultaneously added to the suspension containing the positive electrode material, and reacted for 1.5-3 hours to obtain the modified positive electrode particles; Wherein, when the P in the suspension 2 S 5 When the content of is excessive, the amount of Li added to the suspension per unit time 2 S and P 2 S 5 The molar ratio of 1-2:1 gradually increases to 2.8-3.2:1; or When the Li in the suspension 2 When the content of S is excessive, the amount of Li added to the suspension per unit time is 2 S and P 2 S 5 The molar ratio gradually decreased from 6-9:1 to 2.8-3.2:
1.
14. The method according to claim 13, in, The method further comprises: dispersing the positive electrode material in a first organic solvent to obtain a suspension of the positive electrode material.
15. The method according to claim 14, in, The method further comprises: 2 S is dissolved in the second organic solvent to obtain Li 2 S solution.
16. The method according to claim 15, in, The method further comprises: 2 S 5 Dissolved in a third organic solvent to obtain P 2 S 5 Solution.
17. The method according to claim 16, in, The first organic solvent, the second organic solvent and the third organic solvent are each independently selected from at least one of toluene, xylene, trimethylolbenzene, acetonitrile, tetrahydrofuran, anisole, n-heptane and n-decane.
18. The method according to any one of claims 13 to 17, in, The positive electrode material is coated or uncoated Li(Ni m Co n Mn 1-m-n ) 2 , where 0≤m≤1, 0≤n≤1, and m+n≤1.
19. The method according to claim 18, in, When the positive electrode material is coated Li(Ni m Co n Mn 1-m-n ) 2 When coated on the Li(Ni m Co n Mn 1-m-n ) 2 The surface coating layer is selected from at least one of lithium niobate, lithium titanate, lithium zirconate and lithium phosphate.
20. The method according to claim 19, in, The particle size D50 of the positive electrode material is 3-15 μm.
21. A modified positive electrode particle for a lithium battery prepared according to the method according to any one of claims 13 to 20.
22. A lithium battery positive electrode, comprising a positive electrode current collector and a positive electrode material layer coated on the surface of the positive electrode current collector, It is characterized in that The positive electrode material layer comprises a conductive agent, a first binder, and the modified positive electrode particles according to any one of claims 1 to 12 and 21.
23. The lithium battery positive electrode according to claim 22, in, The conductive agent is selected from at least one of graphite, acetylene black, graphene and carbon black.
24. The lithium battery positive electrode according to claim 22 or 23, in, The first adhesive is a fluorine-containing resin and / or a polyolefin compound.
25. The lithium battery positive electrode according to claim 24, in, The first adhesive is at least one of polyvinylidene fluoride, polytetrafluoroethylene, nitrile rubber and styrene butadiene rubber.
26. An all-solid-state lithium battery, It is characterized in that It comprises a positive electrode, a negative electrode and a solid electrolyte layer, wherein the positive electrode is the positive electrode of a lithium battery as described in any one of claims 22-24.
27. The all-solid-state lithium battery according to claim 26, in, The solid electrolyte layer consists of a solid electrolyte and a second adhesive.
28. The all-solid-state lithium battery according to claim 27, in, The solid electrolyte is selected from Li x M y P z S w and / or doped Li x M y P z S w ; wherein, M is selected from one or more of Si, Ge and Sn, x+4y+5z=2w, 0≤y≤1.5, x>0, z>0, w>0.
29. The all-solid-state lithium battery according to claim 28, in, The solid electrolyte is selected from Li x M y P z S w ; wherein, M is selected from one or more of Si, Ge and Sn, x+4y+5z=2w, 0≤y≤1.5, x>0, z>0, w>0.
30. The all-solid-state lithium battery according to any one of claims 27 to 29, in, The second adhesive is selected from at least one of polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polystyrene, polybutadiene, acrylic resin, epoxy resin, polyethylene oxide, sodium carboxymethyl cellulose and styrene-butadiene latex.