Regeneration method of inner wall components

By using masking parts and sandblasting treatment technology on the inner wall members of the plasma treatment device, the problem of difficulty in maintaining the thickness of the spray coating is solved, and the anodic oxide film area is prevented and the generation of foreign matter is achieved, and the stable regeneration of the spray coating is achieved.

CN115803469BActive Publication Date: 2024-11-01HITACHI HIGH TECH CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202180008331.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-06-28
Publication Date
2024-11-01
Estimated Expiration
2041-06-28

AI Technical Summary

Technical Problem

In the prior art, it is difficult to maintain the thickness of the spray coating during the regeneration of the inner wall member of the plasma treatment device, resulting in a decrease in the anodic oxide film area and the generation of foreign matter.

Method used

By covering the anodic film with a mask on the inner wall member of the plasma treatment device and sandblasting to remove part of the sprayed film, leaving the uncovered anodic film, and then forming a new sprayed film under the mask, ensuring that the anodic film is ensured. The end position of the oxide film remains unchanged, so that the spray coating film is not repeated lamination.

Benefits of technology

The thickness of the spray coating film is fixed, prevents the reduction of the anodic oxide film area and suppresses the generation of foreign matter in the treatment room.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115803469B_ABST
    Figure CN115803469B_ABST
Patent Text Reader

Abstract

An inner wall member (40) provided on the inner wall of a treatment chamber for plasma treatment comprises: a substrate (41); an anodic oxide film (42a) having an end (EP1); and a sprayed film (42b) having an end (EP2). The substrate (41) has a surface (FS1), a surface (FS2) located at a position higher than the surface (FS1), and a side surface (SS1). The regeneration method of the inner wall member (40) has the following steps: (a) covering the anodized film (42a) exposed from the sprayed film (42b) with a masking member (100); (b) removing the sprayed film (42b) on the surface (FS2) by sandblasting the sprayed film (42b), leaving a portion of the sprayed film (42b) on the surface (FS1) and the side (SS1), so that the anodized film (42a) not covered by the masking member (100) is covered by the sprayed film (42b); (c) forming a new sprayed film (42b) on the remaining sprayed film (42b) and the surface (FS2) by spraying; (d) removing the masking member (100).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for regenerating an inner wall member, and in particular to a method for regenerating an inner wall member of an inner wall of a processing chamber for performing plasma processing in a plasma processing device. Background Art

[0002] In the past, in the process of processing semiconductor wafers and manufacturing electronic devices, integrated circuits were formed by stacking multiple film layers on the surface of the semiconductor wafer. In this manufacturing process, fine processing is required, and etching using plasma is used. In such processing by plasma etching, high precision and high yield are required as electronic devices become more integrated.

[0003] A plasma processing device for performing plasma etching treatment has a processing chamber for forming plasma inside a vacuum container, and a semiconductor wafer is stored inside the processing chamber. The components constituting the inner wall of the processing chamber are usually made of metal materials such as aluminum or stainless steel as a base material for reasons related to strength and manufacturing cost. Furthermore, the inner wall of the processing chamber is in contact with the plasma or faces the plasma during the plasma treatment. Therefore, in the components constituting the inner wall of the processing chamber, a film with high plasma resistance is arranged on the surface of the base material. The base material is protected from the plasma by the above-mentioned film.

[0004] As a technique for forming such a film, a method of forming a sprayed film by a so-called spraying method has been known in the past. In the spraying method, plasma is formed in the air or in a gas atmosphere set to a given pressure, and particles of a material for the film are introduced into the plasma to form particles in a semi-molten state. The semi-molten particles are sprayed or irradiated onto the surface of the substrate to form a sprayed film.

[0005] As the material of the sprayed film, a ceramic material such as aluminum oxide, yttrium oxide or yttrium fluoride or a material containing them is used. By covering the surface of the substrate with such a film (sprayed film) to form the inner wall of the processing chamber, the consumption caused by plasma is suppressed for a long period of time, and the amount of interaction between plasma and the surface of the component and the change in properties are suppressed.

[0006] For example, a member of the inner wall of a processing chamber having such a plasma-resistant film is disclosed in Patent Document 1. Patent Document 1 discloses yttrium oxide as an example of the above-mentioned film.

[0007] On the other hand, there are the following problems: the surface of the sprayed film deteriorates after long-term use, the particles of the sprayed film are consumed due to the interaction with the plasma, and the film thickness of the sprayed film decreases. If the surface of the substrate is exposed inside the processing chamber, the particles of the metal material constituting the substrate will adhere to the wafer being processed inside the processing chamber, which may cause contamination on the wafer. Therefore, the following operation is performed on the surface of a component with a sprayed film that has deteriorated, damaged or consumed due to use: the sprayed film is regenerated by the spraying method again.

[0008] Prior art literature

[0009] Patent Literature

[0010] Patent Document 1: JP-A-2004-100039 Summary of the invention

[0011] Problems to be solved by the invention

[0012] However, in the prior art, since the following points are not sufficiently considered, various problems arise.

[0013] For example, in the prior art, when a thermally sprayed film is regenerated by thermal spraying on a deteriorated thermally sprayed film, it is difficult to keep the thickness of the thermally sprayed film constant before and after the re-thermal spraying.

[0014] In addition, when the substrate is aluminum or its alloy, a corrosion-resistant aluminum film (anodized film) formed by anodizing and a film (sprayed film) formed by a spraying method are provided on the surface of the substrate. Then, a boundary is formed between the anodized film and the sprayed film. That is, a sprayed film is formed on the anodized film so that it covers the end of the anodized film. In this case, since the anodized film covered by the sprayed film is also removed when the degraded sprayed film is removed, the position of the end of the anodized film is retreated. Therefore, since the position of the end of the anodized film will retreat each time the sprayed film is repeatedly regenerated, the area of ​​the anodized film is reduced.

[0015] On the other hand, when the sprayed film is removed while leaving the end of the anodized film, the old sprayed film that has deteriorated or consumed will be left on the anodized film. Therefore, every time the regeneration of the sprayed film is repeated, the remaining old sprayed film will be stacked. Since such a stack of old sprayed films is easy to peel off, the stack may become a source of foreign matter inside the processing chamber.

[0016] The main purpose of the present application is to provide a technology for maintaining a constant thickness of a sprayed film before and after re-spraying. In addition, another purpose of the present application is to provide a technology that can prevent the reduction of the area of ​​the anodized film and can suppress the generation of foreign matter inside the processing chamber.

[0017] Other objects and novel features will become apparent from the description of this specification and the accompanying drawings.

[0018] Means for solving problems

[0019] The outline of a typical embodiment among the embodiments disclosed in the present application will be briefly described as follows.

[0020] A method for regenerating an inner wall member in one embodiment is a method for regenerating an inner wall member provided on an inner wall of a processing chamber for performing plasma processing in a plasma processing device. The inner wall member comprises: a substrate having a first surface, a second surface located at a position higher than the first surface, and a first side surface connecting the first surface and the second surface; an anodized film formed on the first surface and the first side surface and having a first end located on the first side surface; and a first sprayed film formed on the first surface, the first side surface, and the second surface so as to cover the first end, the first sprayed film having a second end located on the anodized film formed on the first surface. In addition, the regeneration method of the inner wall member has the following steps: (a) covering the anodized film exposed from the first sprayed film with a masking member; (b) after the step (a), removing the first sprayed film on the second surface by sandblasting the first sprayed film, and leaving a portion of the first sprayed film on the first surface and the first side surface, so that the anodized film not covered by the masking member is covered by the first sprayed film; (c) after the step (b), forming a second sprayed film on the remaining first sprayed film and the second surface by spraying; (d) after the step (c), removing the masking member.

[0021] A method for regenerating an inner wall member in one embodiment is a method for regenerating an inner wall member provided on an inner wall of a processing chamber for performing plasma processing in a plasma processing device. The inner wall member comprises: a substrate having a first surface, a second surface located at a position higher than the first surface, and a first side surface connecting the first surface and the second surface; an anodized film formed on the first surface, the first side surface, and the second surface, and having a first end located on the first surface; and a first sprayed film formed on the first surface so as to cover the first end, the first sprayed film having a second end located on the anodized film formed on the first surface. In addition, the regeneration method of the inner wall member has the following steps: (a) covering the anodized film exposed from the first sprayed film and formed on at least the first surface and the first side surface with a mask; (b) after the step (a), removing the first sprayed film on the first surface by sandblasting the first sprayed film; (c) after the step (b), forming a second sprayed film on the first surface exposed from the mask by spraying; (d) after the step (c), removing the mask.

[0022] Effects of the Invention

[0023] According to one embodiment, the thickness of the thermally sprayed film can be kept constant before and after the re-spraying. In addition, the reduction in the area of ​​the anodized film can be prevented, and the generation of foreign matter inside the processing chamber can be suppressed. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a schematic diagram showing the plasma processing apparatus in the first embodiment.

[0025] Figure 2 This is a conceptual diagram showing the inner wall member in the first embodiment.

[0026] Figure 3 It is a top view showing the inner wall member in Embodiment 1.

[0027] Figure 4 This is a cross-sectional view showing the inner wall member in Embodiment 1.

[0028] Figure 5A This is a cross-sectional view showing a base material of the inner wall member in the first embodiment.

[0029] Figure 5B This is a cross-sectional view showing the regeneration method of the inner wall member in the first embodiment.

[0030] Figure 5C It means next Figure 5B A cross-sectional view of a method for regenerating an inner wall member.

[0031] Figure 5D It means next Figure 5C A cross-sectional view of a method for regenerating an inner wall member.

[0032] Fig. 6A This is a cross-sectional view showing a base material of the inner wall member in the second embodiment.

[0033] Figure 6B This is a cross-sectional view showing a mask member in the second embodiment.

[0034] Figure 6C This is a cross-sectional view showing a method for regenerating an inner wall member in the second embodiment.

[0035] Fig.6D It means next Figure 6C A cross-sectional view of a method for regenerating an inner wall member.

[0036] Fig. 6E It means next Fig.6D A cross-sectional view of a method for regenerating an inner wall member. DETAILED DESCRIPTION

[0037] The following detailed description of the embodiment is based on the accompanying drawings. In addition, in all the figures used to illustrate the embodiment, the same reference numerals are used to mark the components with the same functions, and their repeated descriptions are omitted. In addition, in the following embodiments, the description of the same or identical parts is not repeated in principle except when it is particularly necessary.

[0038] In addition, the X direction, Y direction, and Z direction described in the present application intersect each other and are orthogonal to each other. The expression "planar view" used in the present application means viewing a plane consisting of the X direction and the Y direction from the Z direction.

[0039] (Implementation Method 1)

[0040] <Structure of Plasma Processing Device>

[0041] The following uses Figure 1 The outline of the plasma processing apparatus 1 in the first embodiment will be described.

[0042] The plasma processing apparatus 1 includes a cylindrical vacuum container 2, a processing chamber 4 provided inside the vacuum container 2, and a stage 5 provided inside the processing chamber 4. The upper portion of the processing chamber 4 constitutes a space where plasma 3 is generated, that is, a discharge chamber.

[0043] A window member 6 formed in a disk shape and a plate 7 formed in a disk shape are provided above the stage 5. The window member 6 is made of a dielectric material such as quartz or ceramic, and hermetically seals the interior of the processing chamber 4. The plate 7 is provided below the window member 6 separately from the window member 6, and is made of a dielectric material such as quartz. In addition, a plurality of through holes 8 are provided in the plate 7. A gap 9 is provided between the window member 6 and the plate 7, and a processing gas is supplied to the gap 9 when plasma processing is performed.

[0044] The stage 5 is used to place the wafer WF when plasma processing is performed on the wafer (substrate) WF as the workpiece. In addition, the wafer WF is composed of a semiconductor material such as silicon. The stage 5 is a member whose central axis in the vertical direction is arranged at a position that is concentric with the discharge chamber of the processing chamber 4 or approximately concentric with the discharge chamber of the processing chamber 4 when viewed from above, and is formed in a cylindrical shape.

[0045] The space between the stage 5 and the bottom surface of the processing chamber 4 is connected to the space above the stage 5 via the gap between the side wall of the stage 5 and the side surface of the processing chamber 4. Therefore, the product generated during the processing of the wafer WF placed on the stage 5, the plasma 3 or the gas particles are discharged to the outside of the processing chamber 4 via the space between the stage 5 and the bottom surface of the processing chamber 4.

[0046] Although not shown in detail, the stage 5 is formed in a cylindrical shape and has a base material made of a metal material. The upper surface of the base material is covered with a dielectric film. A heater is provided inside the dielectric film, and a plurality of electrodes are provided above the heater. A DC voltage is supplied to the plurality of electrodes. By this DC voltage, an electrostatic force for adsorbing the wafer WF to the upper surface of the dielectric film and holding the wafer WF can be generated inside the dielectric film and the wafer WF. In addition, the plurality of electrodes are point-symmetrically arranged around the central axis of the stage 5 in the vertical direction, and voltages of different polarities are applied to the plurality of electrodes.

[0047] Furthermore, multiple cooling medium flow paths arranged concentrically or spirally are provided on the stage 5. Furthermore, in a state where the wafer WF is placed on the upper surface of the dielectric film, a gas having heat transfer properties such as helium (He) is supplied to the gap between the lower surface of the wafer WF and the upper surface of the dielectric film. Therefore, a pipe for circulating the gas is arranged inside the substrate and the dielectric film.

[0048] In addition, the plasma processing apparatus 1 includes an impedance matching box 10 and a high-frequency power supply 11. The substrate on the stage 5 is connected to the high-frequency power supply 11 via the impedance matching box 10. In the plasma processing of the wafer WF, in order to form an electric field for guiding charged particles in the plasma onto the upper surface of the wafer WF, high-frequency power is supplied from the high-frequency power supply 11 to the substrate.

[0049] In addition, the plasma processing device 1 includes a waveguide 12, a magnetron oscillator 13, a solenoid coil 14, and a solenoid coil 15. The waveguide 12 is provided above the window member 6, and the magnetron oscillator 13 is provided at one end of the waveguide 12. The magnetron oscillator 13 can oscillate and output the electric field of microwaves. The waveguide 12 is a pipeline for propagating the electric field of microwaves, and the electric field of microwaves is supplied to the inside of the processing chamber 4 via the waveguide 12. The solenoid coil 14 and the solenoid coil 15 are provided around the waveguide 12 and the processing chamber 4, and are used as a magnetic field generating unit.

[0050] In addition, the waveguide 12 includes a square waveguide portion and a circular waveguide portion. The square waveguide portion has a rectangular cross-sectional shape and extends in the horizontal direction. A magnetron oscillator 13 is provided at one end of the square waveguide portion. The circular waveguide portion is connected to the other end of the square waveguide portion. The circular waveguide portion has a circular cross-sectional shape and is configured such that the central axis extends in the vertical direction.

[0051] In addition, the plasma processing apparatus 1 includes a pipe 16 and a gas supply device 17. The gas supply device 17 is connected to the processing chamber 4 via the pipe 16. The processing gas is supplied from the gas supply device 17 to the gap 9 via the pipe 16 and diffused inside the gap 9. The diffused processing gas is supplied from the through hole 8 to the top of the stage 5.

[0052] In addition, the plasma processing device 1 includes a pressure adjustment plate 18, a pressure detector 19, a turbomolecular pump 20 as a high vacuum pump, a dry pump 21 as a roughing pump, an exhaust pipe 22, and valves 23 to 25. The space between the carrier 5 and the bottom surface of the processing chamber 4 functions as a vacuum exhaust section. The pressure adjustment plate 18 is a disc-shaped valve that increases or decreases the area of ​​the flow path for gas to flow into the exhaust port by moving up and down above the exhaust port. That is, the pressure adjustment plate 18 also serves as a valve for opening and closing the exhaust port.

[0053] The pressure detector 19 is a sensor for detecting the pressure inside the processing chamber 4. The signal output from the pressure detector 19 is sent to a control unit (not shown), and the value of the pressure is detected in the control unit, and a command signal is output from the control unit according to the detected value. The pressure adjustment plate 18 is driven based on the command signal, and the position of the pressure adjustment plate 18 in the vertical direction changes, thereby increasing or decreasing the area of ​​the exhaust flow path.

[0054] The outlet of the turbomolecular pump 20 is connected to the dry pump 21 via a pipe, and a valve 23 is provided in the middle of the pipe. The space between the stage 5 and the bottom surface of the processing chamber 4 is connected to the exhaust pipe 22, and the exhaust pipe 22 is provided with a valve 24 and a valve 25. The valve 24 is a valve for slow exhaust for exhausting the processing chamber 4 from atmospheric pressure to a vacuum state by exhausting the dry pump 21 at a low speed, and the valve 23 is a valve for main exhaust for exhausting the processing chamber 4 at a high speed by the turbomolecular pump 20.

[0055] <Plasma treatment>

[0056] Hereinafter, as an example of plasma processing, a case where an etching process using plasma 3 is performed on a predetermined film formed in advance on the upper surface of the wafer WF will be described.

[0057] The wafer WF is loaded on the front end of the arm of a vacuum transport device such as a robot arm from the outside of the plasma processing apparatus 1, transported to the inside of the processing chamber 4, and placed on the stage 5. When the arm of the vacuum transport device is withdrawn from the processing chamber 4, the inside of the processing chamber 4 is sealed. Then, a DC voltage is applied to the electrode for electrostatic attraction inside the dielectric film of the stage 5, and the wafer WF is held on the dielectric film by the generated electrostatic force.

[0058] In this state, a gas having heat transfer properties such as helium (He) is supplied to the gap between the wafer WF and the dielectric film via a pipe provided inside the stage 5. In addition, a coolant adjusted to a given temperature by a coolant temperature adjuster (not shown) is supplied to the coolant flow path inside the stage 5. Thus, heat transfer is promoted between the substrate whose temperature is adjusted and the wafer WF, and the temperature of the wafer WF is adjusted to a value within a range suitable for the start of plasma processing.

[0059] The processing gas whose flow rate and speed are adjusted by the gas supply device 17 is supplied to the inside of the processing chamber 4 through the pipe 16, and the inside of the processing chamber 4 is exhausted from the exhaust port by the operation of the turbomolecular pump 20. The pressure inside the processing chamber 4 is adjusted to a value within a range suitable for plasma processing by the balance between the two.

[0060] In this state, the electric field of microwaves is oscillated from the magnetron oscillator 13. The electric field of microwaves propagates inside the waveguide 12, passing through the window member 6 and the plate 7. Furthermore, the magnetic field generated by the solenoid coil 14 and the solenoid coil 15 is supplied to the processing chamber 4. Electron cyclotron resonance (ECR) is caused by the interaction between the above magnetic field and the electric field of microwaves. Then, plasma 3 is generated inside the processing chamber 4 by exciting, ionizing or dissociating atoms or molecules of the processing gas.

[0061] When the plasma 3 is generated, high-frequency power is supplied from the high-frequency power supply 11 to the substrate of the stage 5, a bias potential is formed on the upper surface of the wafer WF, and charged particles such as ions in the plasma 3 are guided to the upper surface of the wafer WF. Thus, etching processing is performed on a given film of the wafer WF along the pattern shape of the mask layer. Afterwards, when it is detected that the processing of the film to be processed has reached its end point, the supply of high-frequency power from the high-frequency power supply 11 is stopped, and the plasma processing is stopped.

[0062] When no further etching of the wafer WF is required, high vacuum evacuation is performed. Then, after static electricity is removed to release the adsorption of the wafer WF, the arm of the vacuum transport device enters the processing chamber 4 to transport the processed wafer WF to the outside of the plasma processing device 1.

[0063] <Inner wall member of processing chamber>

[0064] like Figure 1 As shown, an inner wall member 40 is provided inside the processing chamber 4. The inner wall member 40 functions as, for example, a ground electrode for stabilizing the potential of the plasma 3 which is a dielectric.

[0065] like Figure 2 As shown, the inner wall member 40 includes a base material 41 and a film 42 covering the surface of the base material 41. The base material 41 is made of a conductive material, for example, a metal material such as aluminum, an aluminum alloy, stainless steel, or a stainless steel alloy.

[0066] The inner wall member 40 is exposed to the plasma 3 during the plasma treatment. If the film 42 is not formed on the surface of the substrate 41, the substrate 41 becomes a source of corrosion or foreign matter due to the exposure of the substrate 41 to the plasma 3, and may contaminate the wafer WF. The film 42 is provided to suppress the contamination of the wafer WF, and is made of a material having a higher resistance to the plasma 3 than the substrate 41. The film 42 can maintain the function of the inner wall member 40 as a ground electrode, and can protect the substrate 41 from the plasma 3.

[0067] In addition, metal materials such as stainless steel alloys and aluminum alloys are also used for the substrate 30 that does not function as a ground electrode. Therefore, the surface of the substrate 30 is also treated to improve the resistance to the plasma 3 or to reduce the consumption of the substrate 30 in order to suppress corrosion or generation of foreign matter due to exposure to the plasma 3. Such treatment is, for example, passivation treatment, formation of a thermal spray film, or film formation by a PVD method or a CVD method.

[0068] Although not shown, in order to reduce the consumption of the substrate 30 caused by the plasma 3, a cylindrical cover made of ceramics such as yttrium oxide or quartz may be arranged inside the inner wall of the cylindrical substrate 30. By arranging such a cover between the substrate 30 and the plasma 3, the contact between the substrate 30 and the highly reactive particles in the plasma 3 or the collision between the substrate 30 and the charged particles is blocked or reduced. Thus, the consumption of the substrate 30 can be suppressed.

[0069] use Figure 3 as well as Figure 4 The structure of the inner wall member 40 will be described. Figure 3 is a top view showing the inner wall member 40, Figure 4 It is along Figure 3 A cross-sectional view along line AA is shown.

[0070] The inner wall member 40 (base material 41) is generally formed into a cylindrical shape having a given thickness between the inner periphery and the outer periphery. In addition, the inner wall member 40 is composed of an upper portion 40a, an intermediate portion 40b, and a lower portion 40c. The upper portion 40a is a portion where the inner diameter and outer diameter of the cylinder are relatively small, and the lower portion 40c is a portion where the inner diameter and outer diameter of the cylinder are relatively large. The intermediate portion 40b is a portion for connecting the upper portion 40a and the lower portion 40c, and forms a truncated cone shape in which the inner diameter and outer diameter of the cylinder continuously change.

[0071] The inner wall member 40 is provided along the inner wall of the processing chamber 4 so as to surround the outer periphery of the stage 5. A sprayed film is formed by a spraying method on the inner peripheral surface of the inner wall member 40 (the inner peripheral surface of the substrate 41) as a part of the film 42. In addition, when the inner wall member 40 is installed inside the processing chamber 4, an anodic oxide film is formed by anodizing treatment on the outer peripheral surface of the inner wall member 40 (the outer peripheral surface of the substrate 41) as a part of the film 42.

[0072] In addition, the sprayed film is formed not only on the surface of the inner peripheral side of the substrate 41, but also on the surface of the outer peripheral side of the substrate 41 through the upper end of the upper portion 40a. The reason is that the particles of the plasma 3 are wound from the inner peripheral side of the inner wall member 40 to the outer peripheral side of the inner wall member 40 at the upper portion 40a, and there is a possibility of interaction with the surface of the outer peripheral side of the substrate 41. Therefore, it is necessary to form the sprayed film on the surface of the outer peripheral side of the substrate 41 until the area where the particles of the plasma 3 are expected to be wound. Figure 4 Such a region is shown as region 50 .

[0073] Figure 5A to Figure 5D It is a cross-sectional view showing an enlarged region 50. The inner wall member 40 in the first embodiment includes a base material 41, an anodic oxide film 42a, and a thermal spray film 42b as described below. Figure 5A4 shows the substrate 41 before the film 42 (anodized film 42a, sprayed film 42b) is formed. Figure 5B The substrate 41 after the film 42 is formed is shown.

[0074] like Figure 5A As shown in the figure, in the substrate 41 in the first embodiment, a height difference is generated in the direction (X direction) from the inner peripheral side of the inner wall member 40 (the inner peripheral side of the substrate 41) to the outer peripheral side of the inner wall member 40 (the outer peripheral side of the substrate 41). That is, the substrate 41 has: a surface FS1; a surface FS2 located at a position higher than the surface FS1; and a side surface SS1 connecting the surface FS1 and the surface FS2. In addition, the distance L1 between the surface FS1 and the surface FS2 is equivalent to the height of the height difference and the length of the side surface SS1. Here, the distance L1 is, for example, 0.5 mm.

[0075] like Figure 5B As shown, the anodized film 42a is formed on the surface FS1 and on the side SS1. In addition, the anodized film 42a has an end EP1 located on the side SS1. The anodized film 42a is formed by anodizing before forming the sprayed film 42b. When the substrate 41 is, for example, aluminum or an aluminum alloy, the anodized film 42a is a corrosion-resistant aluminum film.

[0076] The sprayed film 42b is formed on the surface FS1, the side surface SS1, and the surface FS2 so as to cover the end EP1. In addition, the sprayed film 42b has an end EP2 located on the anodized film 42a formed on the surface FS1.

[0077] The sprayed film 42b is formed, for example, by a plasma spraying method. In the spraying method, plasma is formed under atmospheric pressure, and particles of yttrium oxide, yttrium fluoride, or a material containing them are supplied into the plasma to make the particles semi-molten. The semi-molten particles are sprayed or irradiated onto the surfaces FS1 and FS2 of the substrate 41, thereby forming the sprayed film 42b.

[0078] The surface irregularities of the thermal spray film 42b are configured such that the arithmetic mean roughness (surface roughness) Ra is, for example, 8 or less. The average size (average particle diameter) of each particle of the thermal spray film 42b is, for example, 10 μm to 50 μm at volume-based D50.

[0079] In the region 50, the surface FS1, the side surface SS1, and the surface FS2 of the substrate 41 are covered by at least one of the anodized film 42a and the sprayed film 42b, thereby preventing the substrate 41 from being exposed to the plasma 3 during the plasma treatment.

[0080] <Method for Regenerating Inner Wall Member in Embodiment 1>

[0081] The following uses Figure 5B to Figure 5D Each step included in the method for regenerating the inner wall member 40 (the method for manufacturing the inner wall member 40 ) will be described.

[0082] Figure 5B The inner wall member 40 is arranged in the processing chamber 4 for a given period and is exposed to the plasma 3. Since the thermal sprayed film 42b exposed to the plasma 3 is modified or consumed, it is necessary to remove the thermal sprayed film 42b and regenerate the thermal sprayed film 42b.

[0083] First, if Figure 5C As shown, the anodized film 42a exposed from the thermal spray film 42b is covered with a mask 100. At this time, the mask 100 is in contact with the end EP2 of the thermal spray film 42b. The mask 100 is made of a material having a property that it will not be removed by the sandblasting process described later, such as a resin tape.

[0084] Next, the sprayed film 42b is subjected to sandblasting. The sandblasting is performed by projecting sandblasting particles 200 from the direction from the surface FS2 to the surface FS1 and in a direction inclined at a given angle θ relative to the surface FS1. The sandblasting particles 200 collide with particles of the sprayed film 42b, and the sprayed film 42b is removed by physical action. In addition, by appropriately selecting the angle θ of the projected sandblasting particles 200, a portion of the sprayed film 42b can be left.

[0085] By such sandblasting, the sprayed film 42b on the surface FS2 is removed, and a portion of the sprayed film 42b on the surface FS1 and the side surface SS1 is left, so that the sprayed film 42b covers the anodized film 42a that is not covered by the mask 100. In this way, since the anodized film 42a is covered by either the remaining sprayed film 42b or the mask 100, the entire anodized film 42a is not exposed to the sandblasting.

[0086] Next, if Figure 5D As shown in FIG. 1 , a new sprayed film 42b is formed on the remaining sprayed film 42b and on the surface FS2 by spraying. The method and conditions for forming the new sprayed film 42b are the same as those in FIG. Figure 5B The method described in the above is the same. In addition, the direction in which the semi-molten particles 300 are sprayed onto the surfaces FS1 and FS2 of the substrate 41 is perpendicular to the surfaces FS1 and FS2. Next, the mask 100 is removed. In this way, the sprayed film 42b can be regenerated, so the inner wall member 40 is sprayed onto the inner wall member 40. Figure 5B state of regeneration.

[0087] in addition, Figure 5DThe newly formed sprayed film 42b has an end EP3 located on the anodized film 42a formed on the surface FS1. Figure 5B The position of the end EP2 of the sprayed film 42b is consistent.

[0088] In addition, the initially formed thermal spray film 42b and the newly formed thermal spray film 42b are made of the same material. The thermal spray film 42b remaining after the sandblasting process is a part that is not directly exposed to the plasma 3 during the plasma treatment and is almost not modified. Therefore, the remaining thermal spray film 42b and the new thermal spray film 42b are integrated as the same high-quality thermal spray film 42b.

[0089] Afterwards, when the inner wall member 40 is exposed to the plasma 3 again and the thermal sprayed film 42b is modified, the thermal spraying is repeated. Figure 5B to Figure 5D Each process can regenerate the sprayed film 42b and regenerate the inner wall component 40.

[0090] As described above, in the prior art, since the position of the end EP1 of the anodized film 42a retreats each time the regeneration of the sprayed film 42b is repeated, there is a problem that the area of ​​the anodized film 42a is reduced. In addition, when the sprayed film 42b is removed so that the end EP1 of the anodized film 42a is left, each time the regeneration of the sprayed film 42b is repeated, the remaining old sprayed film 42b is stacked, and there is a problem that the stacked body becomes a source of foreign matter inside the processing chamber.

[0091] In contrast, according to Embodiment 1, the position of the end EP1 of the anodized film 42a does not change before and after the regeneration of the sprayed film 42b. Therefore, the reduction in the area of ​​the anodized film 42a can be prevented, and the generation of foreign matter inside the processing chamber 4 can be suppressed. In addition, Figure 5D The position of the end EP3 of the newly formed sprayed film 42b is Figure 5B That is, it is possible to provide a thermal spray film 42b having substantially the same parameters as before and after the thermal spraying, such as thickness and area.

[0092] (Implementation Method 2)

[0093] The following uses Figure 6A to Figure 6E The inner wall member 40 and the regeneration method of the inner wall member 40 (the manufacturing method of the inner wall member 40) in Embodiment 2 will be described. In the following description, the differences from Embodiment 1 will be mainly described, and the description of the points overlapping with Embodiment 1 will be omitted.

[0094] <Inner Wall Member in Embodiment 2>

[0095] Figure 6A to Figure 6E Is magnification Figure 4 The inner wall member 40 in the second embodiment also includes a substrate 41, an anodic oxide film 42a and a sprayed film 42b as in the first embodiment. The materials constituting these and the method for forming these are the same as in the first embodiment.

[0096] Fig. 6A 4 shows the substrate 41 before the film 42 (anodized film 42a, sprayed film 42b) is formed. Figure 6B The masking member 101 used in the second embodiment is shown. Figure 6C The substrate 41 after the film 42 is formed is shown.

[0097] like Fig. 6A As shown, in the substrate 41 in Embodiment 2, a height difference is also generated in the direction (X direction) from the inner peripheral side of the inner wall member 40 (the inner peripheral side of the substrate 41) to the outer peripheral side of the inner wall member 40 (the outer peripheral side of the substrate 41). In addition, the distance L2 between the surface FS1 and the surface FS2 is equivalent to the height of the height difference and the length of the side surface SS1. Here, the distance L2 is, for example, 5.0 mm.

[0098] like Figure 6B As shown, the mask 101 in Embodiment 2 is an L-shaped metal member prefabricated to match the shape of the height difference. That is, the mask 101 is a fixture having a shape along the surface FS1 and the side SS1, respectively, and is made of a metal material. The distance L3 of the portion along the side SS1 of the mask 101 is designed to be slightly smaller than the distance L2, for example, 4.5 mm. The portion along the surface FS1 of the mask 101 is designed to be closer to the side SS1 than the end EP1 of the anodized film 42a, for example, 2.0 mm. The thickness L5 of the mask 101 is, for example, 1.0 mm.

[0099] like Figure 6C As shown in the figure, the anodized film 42a in the second embodiment is formed on the surface FS1, on the side surface SS1, and on the surface FS2. In addition, the anodized film 42a has an end EP1 located on the surface FS1. The sprayed film 42b is formed on the surface FS1 so as to cover the end EP1. In addition, the sprayed film 42b has an end EP2 located on the anodized film 42a formed on the surface FS1.

[0100] In the second embodiment, the surface FS1, the side surface SS1 and the surface FS2 of the substrate 41 in the region 50 are also covered by at least one of the anodized film 42a or the sprayed film 42b, thereby preventing the substrate 41 from being exposed to the plasma 3 during the plasma treatment.

[0101] <Method for Regenerating Inner Wall Member in Embodiment 2>

[0102] The following uses Figure 6C to Figure 6E Each step included in the method for regenerating the inner wall member 40 (the method for manufacturing the inner wall member 40 ) will be described.

[0103] Figure 6C The inner wall member 40 is arranged in the processing chamber 4 during a given period and is exposed to the plasma 3. Since the sprayed film 42b exposed to the plasma 3 is modified or consumed, it is necessary to remove the sprayed film 42b and regenerate the sprayed film 42b.

[0104] First, if Fig.6D As shown, the anodized film 42a exposed from the thermal sprayed film 42b and formed at least on the surface FS1 and the side surface SS1 is covered with a mask 101. At this time, the mask 101 is in contact with the end EP2 of the thermal sprayed film 42b.

[0105] Next, the sprayed film 42b is sandblasted to remove the sprayed film 42b on the surface FS1. The sandblasting is performed by projecting sandblasting particles 200 from a direction perpendicular to the surface FS1. The sandblasting particles 200 collide with particles of the sprayed film 42b, and the sprayed film 42b is removed by physical action. The projection range of the sandblasting particles 200 is set on the surface FS1 including the mask 101 so as not to affect the surface FS2.

[0106] Here, the anodized film 42a which is not covered by the mask 101 and is covered by the thermal sprayed film 42b is also removed. Therefore, the position of the end EP1 of the anodized film 42a is slightly retreated and moved to a position matching the mask 101.

[0107] Next, if Fig. 6E As shown in FIG. 1 , a new thermal spray film 42b is formed by thermal spraying on the surface FS1 exposed from the mask 101. The method and conditions for forming the new thermal spray film 42b are the same as those in FIG. Figure 5B The same as described in the above. In addition, the direction in which the semi-molten particles 300 are sprayed onto the surface FS1 of the substrate 41 is perpendicular to the surface FS1. Next, the mask 101 is removed. In this way, in the second embodiment, since the sprayed film 42b can be regenerated, the inner wall member 40 is Figure 6C state of regeneration.

[0108] in addition, Fig. 6E The newly formed sprayed film 42b has an end EP3 located on the anodized film 42a formed on the surface FS1. Figure 6C The position of the end EP2 of the sprayed film 42b is consistent. In addition, the position of the end EP3 is consistent with Fig.6DThe position of the end EP1 of the anodized film 42a which is retreating is also consistent.

[0109] Afterwards, when the inner wall member 40 is exposed to the plasma 3 again and a modification occurs in the sprayed film 42b, the inner wall member 40 can be repeatedly Figure 6C to Figure 6E Through each process, the sprayed film 42b is regenerated and the inner wall component 40 is regenerated.

[0110] In the second embodiment, a jig which is a metal member having a shape along the height difference is used as the mask 101. Therefore, the mask 101 can be quickly installed by only attaching the mask 101 to the surface FS1 and the side surface SS1, that is, only attaching the mask 101 to the height difference. In addition, since the shape of the mask 101 is constant, the position of the end EP1 of the anodized film 42a can be always fixed, and the position of the end EP3 of the newly formed sprayed film 42b can be fixed.

[0111] like Fig.6D As described in the previous section, when the first spray coating 42b is regenerated, the position of the end EP1 of the anodized film 42a is slightly retracted. However, since the shape of the mask 101 is unchanged when the spray coating 42b is regenerated for the second and subsequent times, the position of the end EP1 does not change and is consistent before and after the spray coating. That is, even if the spray coating is repeated, the position of the end EP1 is not changed. Figure 6C to Figure 6E In the case where the regeneration of the sprayed film 42b is repeated in each process, the position of the end EP1 and the position of the end EP3 are always fixed. Therefore, in the second embodiment, it is also possible to prevent the reduction of the area of ​​the anodized film 42a and suppress the generation of foreign matter inside the processing chamber 4. In addition, it is possible to provide a sprayed film 42b having substantially the same various parameters such as thickness and area before and after the re-spraying.

[0112] As mentioned above, although this invention was specifically described based on the said embodiment, this invention is not limited to the said embodiment, Various changes can be made within the range which does not deviate from the summary.

[0113] For example, in the first embodiment, a jig having a constant shape such as the masking member 101 can be used instead of the masking member 100. However, depending on the specifications of the plasma processing device 1, the inner wall member 40 may be formed in various shapes. In this case, it is necessary to prepare jigs corresponding to them. In addition, the portion where the anodized film 42a and the sprayed film 42b are connected is not limited to a portion where it is easy to always set the jig with good accuracy (for example, Fig.6D ) As in the first embodiment, if the masking member 100 is a resin tape, it is not necessary to prepare a new jig, and thus it is easy to apply to the inner wall members 40 of various shapes.

[0114] That is, in terms of the accuracy of aligning the position of the end EP1 of the anodized film 42a and the position of the end EP3 of the new sprayed film 42b and the rapidity of setting the mask, the second embodiment is superior to the first embodiment. On the other hand, in terms of the versatility of the mask, the first embodiment is superior to the second embodiment.

[0115] Description of Reference Numerals

[0116] 1 Plasma treatment device

[0117] 2 Vacuum container

[0118] 3 Plasma

[0119] 4 Processing Chamber

[0120] 5. Carrier

[0121] 6 Window components

[0122] 7 Plates

[0123] 8. Through the Void

[0124] 9 Gap

[0125] 10 Impedance Matching Box

[0126] 11 High frequency power supply

[0127] 12 Waveguide

[0128] 13 Magnetron Oscillator

[0129] 14 Solenoid Coil

[0130] 15 Solenoid Coil

[0131] 16 piping

[0132] 17 Gas supply device

[0133] 18 Pressure adjustment plate

[0134] 19 Pressure detector

[0135] 20 Turbomolecular pump

[0136] 21 Dry Pump

[0137] 22 Exhaust pipe

[0138] 23~25 valves

[0139] 30 Base material

[0140] 40 Inner wall member (ground electrode)

[0141] 40a upper

[0142] 40b Middle

[0143] 40c Lower

[0144] 41 Substrate

[0145] 42 membrane

[0146] 42a Anodic oxide film

[0147] 42b Spray coating

[0148] 50 Areas

[0149] 100 Masking piece (resin tape)

[0150] 101 Masking piece (fixture)

[0151] 200 Sandblasting particles

[0152] 300 Semi-molten particles

[0153] EP1~EP3 end

[0154] FS1, FS2 surface

[0155] SS1 side

[0156] WF wafer (processed part).

Claims

1. A method for regenerating an inner wall member, the method being a method for regenerating an inner wall member provided on the inner wall of a processing chamber for performing plasma processing in a plasma processing device, It is characterized in that The inner wall member comprises: A substrate having a first surface, a second surface located higher than the first surface, and a first side surface connecting the first surface and the second surface; an anodic oxide film formed on the first surface and the first side surface and having a first end portion located on the first side surface; and a first sprayed film formed on the first surface, the first side surface, and the second surface so as to cover the first end, the first sprayed film having a second end located on the anodized film formed on the first surface, The inner wall member regeneration method comprises the following steps: (a) covering the anodized film exposed from the first sprayed film with a mask; (b) after the step (a), the first sprayed film on the second surface is removed by sandblasting, and a portion of the first sprayed film on the first surface and the first side surface is left, so that the anodized film not covered by the mask is covered by the first sprayed film; (c) after the step (b), forming a second sprayed film on the remaining first sprayed film and on the second surface by spraying; (d) After the step (c), the masking member is removed.

2. The method for regenerating an inner wall member according to claim 1, It is characterized in that In the step (b), the blasting treatment is performed by projecting blasting particles from a direction that goes from the second surface to the first surface and is inclined at a given angle with respect to the first surface.

3. The method for regenerating an inner wall member according to claim 1, It is characterized in that In the step (a), the mask is in contact with the second end portion.

4. The method for regenerating an inner wall member according to claim 3, It is characterized in that The second sprayed film has a third end portion located on the anodized film formed on the first surface. The position of the third end portion coincides with the position of the second end portion of the first sprayed film.

5. The method for regenerating an inner wall member according to claim 1, It is characterized in that The masking member is formed of a resin tape.

6. The method for regenerating an inner wall member according to claim 1, It is characterized in that The first sprayed film and the second sprayed film are made of the same material.

7. The method for regenerating an inner wall member according to claim 1, It is characterized in that The substrate is formed into a cylindrical shape having a given thickness between the inner periphery and the outer periphery, The first surface, the first side surface, and the second surface are provided on the outer peripheral side of the substrate.

8. A method for regenerating an inner wall member, the method being a method for regenerating an inner wall member provided on the inner wall of a processing chamber for performing plasma processing in a plasma processing apparatus, It is characterized in that The inner wall member comprises: A substrate having a first surface, a second surface located higher than the first surface, and a first side surface connecting the first surface and the second surface; an anodic oxide film formed on the first surface, the first side surface, and the second surface and having a first end portion located on the first surface; and a first sprayed film formed on the first surface so as to cover the first end, the first sprayed film having a second end located on the anodized film formed on the first surface, The inner wall member regeneration method comprises the following steps: (a) covering the anodized film exposed from the first sprayed film and formed at least on the first surface and the first side surface with a mask; (b) after the step (a), removing the first sprayed film on the first surface by sandblasting the first sprayed film; (c) after the step (b), forming a second sprayed film on the first surface exposed from the mask member by spraying; (d) After the step (c), the masking member is removed.

9. The method for regenerating an inner wall member according to claim 8, It is characterized in that In the step (a), the mask is in contact with the second end portion.

10. The method for regenerating an inner wall member according to claim 9, It is characterized in that The second sprayed film has a third end portion located on the first surface, The position of the third end portion coincides with the position of the second end portion of the first sprayed film.

11. The method for regenerating an inner wall member according to claim 8, It is characterized in that The mask is a jig having a shape along the shapes of the first surface and the first side surface.

12. The method for regenerating an inner wall member according to claim 8, It is characterized in that The first sprayed film and the second sprayed film are made of the same material.

13. The method for regenerating an inner wall member according to claim 8, It is characterized in that The substrate is formed into a cylindrical shape having a given thickness between the inner periphery and the outer periphery, The first surface, the first side surface, and the second surface are provided on the outer peripheral side of the substrate.

14. The method for regenerating an inner wall member according to claim 8, It is characterized in that In the step (b), the anodized film that is not covered by the mask and is covered by the first sprayed film is also removed, and the position of the first end portion is retracted.

15. The method for regenerating an inner wall member according to claim 14, It is characterized in that (e) after the step (d), exposing the inner wall member to plasma; (f) after the step (e), the anodized film exposed from the second sprayed film and formed at least on the first surface and the first side surface is covered with the mask; (g) after the step (f), removing the second sprayed film on the first surface by sandblasting the second sprayed film; (h) after the step (g), forming a third sprayed film on the first surface exposed from the mask member by spraying; (i) after the step (h), removing the masking member; The position of the first end after the step (i) coincides with the position of the first end before the step (f).

Citation Information

Patent Citations

  • Rare earth oxide thermal spraying member and powder for thermal spraying

    JP2004100039A

  • Regeneration method for clean rough surface of part in vacuum coating cavity

    CN105274465A

  • Dry etching machine table inner wallboard regeneration method

    CN107630185A

  • Component for plasma processing device and jet plating method

    CN109256326A

  • Repairing method of surface defect

    CN109622333A