A comprehensive process for recovering high-quality products from tailings

Through flotation and acid separation under different pH conditions, combined with the use of anionic and cationic associates and activators, the problem of flotation separation of feldspar and quartz was successfully solved, and the recovery of high-quality products and the comprehensive utilization of resources were achieved. , avoiding environmental and equipment hazards.

CN115805133BActive Publication Date: 2024-10-18CENT SOUTH UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202111078108.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-09-15
Publication Date
2024-10-18
Estimated Expiration
2041-09-15

AI Technical Summary

Technical Problem

The flotation separation method of feldspar and quartz in the prior art has limitations of being fluorine-free with acid or with fluorine and acid, which results in low comprehensive utilization rate of non-metallic mineral resources in tailings and causes harm to the environment and equipment. There is a lack of fluorine-free technology. Acid-free, green and efficient process.

Method used

The flotation separation of mica and quartz is carried out under the conditions of pH value 10.00-10.60 and 10.60-11.00 respectively, and then the acid separation and impurity removal of quartz is carried out under the condition of pH value 2.70-3.20, using anion and cation association, activation flotation and selection using agents and cationic collectors to obtain high-quality feldspar and quartz products.

Benefits of technology

It achieves efficient recovery of feldspar and quartz in tailings under fluorine-free and acid-free slurry conditions, avoids equipment corrosion and environmental hazards, improves resource utilization, reduces mine tailings emissions, and has high promotion value.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115805133B_ABST
    Figure CN115805133B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of mineral flotation separation, and is a process for comprehensively recovering high-quality products in tailings. The present invention takes tailings as a processing object, first separates mica by flotation under the condition of pH 10.00-10.60, and then separates quartz by flotation under the condition of pH 10.60-11.00; after the quartz flotation is completed, the residue at the bottom of the tank is a feldspar product, and the quartz is selected twice as a foam product under the condition of pH 10.60-11.00, and then acid selection is performed to remove impurities under the condition of pH 2.70-3.20, and finally high-quality feldspar products and quartz products are obtained; the flotation collector for mica separation is an anion-cation association collector; the flotation collector for quartz separation is an anion collector; the flotation collector for quartz impurity removal is a cationic collector. In the flotation separation process of mica, quartz and feldspar in tailings, the reagents used in the method of the present invention can be naturally degraded, so that the pollution to the environment is small and the method is environmentally friendly. In addition, the patented feldspar and quartz flotation separation process of the present invention is fluorine-free and acid-free, and has low requirements for flotation equipment, thereby reducing production costs. Therefore, the present invention is convenient for large-scale industrial application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of mineral flotation, and in particular relates to a process for comprehensively recovering high-quality products from tailings. Background Art

[0002] Due to the characteristics of my country's mineral resources being poor, fine and complex, the current accumulated stockpile of tailings in my country is over 10 billion tons, and is growing at an annual output rate of about 1.2 billion tons, accounting for more than 50% of the world's tailings output, while the comprehensive utilization rate of tailings is only about 13.3%. With the progress of industrial production, tailings have become one of the solid wastes with the lowest comprehensive utilization rate and the largest output in my country.

[0003] my country's mine tailings contain a large amount of non-metallic mineral resources, especially non-ferrous metal tailings in metal mines. A large number of studies have reported that the non-metallic minerals in metal mine tailings are mainly feldspar, quartz and mica, as shown in Table 1. The non-metallic mineral resources accumulated in the tailings ponds of my country's metal mines account for the vast majority of its total tailings resources. The comprehensive utilization of metal mine tailings is of great significance in reducing the waste of mineral resources, reducing the discharge of mine solid wastes, and avoiding excessive mining of non-metallic mines.

[0004] Table 1 Non-metallic components and contents in tailings from different metal mines

[0005]

[0006] However, most of the metal mining enterprises in my country only focus on the secondary recovery of the target metals in the tailings. However, due to the reasons of mineral processing technology and equipment, only a few mines have recovered the valuable components in the tailings. The flotation separation of feldspar and quartz is the most important factor restricting the comprehensive utilization of tailings in my country. At present, the research on the flotation separation of feldspar and quartz in tailings mainly adopts the "fluorine-free acid method" and the "fluorine-containing acid method". Both methods have great harm to the environment and equipment. These factors have largely restricted the comprehensive utilization of non-metallic mineral resources in tailings in actual production.

[0007] Therefore, in order to strengthen the comprehensive utilization of mine tailings and reduce the excessive exploitation of non-metallic mines, it is urgently necessary to develop a set of feldspar and quartz flotation separation processes that are fluorine-free and acid-free, have high industrial feasibility, are complete in process, and are green and efficient, so as to comprehensively recover high-quality feldspar and quartz products from tailings. Summary of the invention

[0008] The technical problem to be solved by the present invention is to overcome the deficiencies and defects of the fluorine-free and acid-free flotation separation technology of feldspar and quartz in the background technology and to solve the problem of comprehensive recovery and utilization of non-metallic minerals in tailings.

[0009] In order to solve the above technical problems, the technical solution proposed by the present invention is:

[0010] The invention discloses a process for comprehensively recovering high-quality products from tailings. The tailings are treated as the processing object, and mica is firstly separated by flotation under the condition of pH 10.00-10.60, and then quartz is separated by flotation under the condition of pH 10.60-11.00. The residue at the bottom of the tank after the quartz flotation is a feldspar product, and the quartz is selected twice as a foam product under the condition of pH 10.60-11.00, and then the quartz is acid-selected and impurities are removed under the condition of pH 2.70-3.20, so as to finally obtain high-quality feldspar products and quartz products. The flotation reagent for mica separation is an anion-cation association collector, the flotation reagent for quartz separation is an activator and an anion collector, and the flotation reagent for quartz acid impurity removal is a cationic collector.

[0011] As a preferred embodiment, the present invention provides a process for comprehensively recovering high-quality products from tailings; the anionic collectors are all fatty acid collectors; and the cationic collectors are all amine collectors.

[0012] As a preferred embodiment; the present invention provides a process for comprehensive recovery of high-quality products from tailings; the anionic collector is selected from at least one of oleic acid, oxidized paraffin soap, and tall oil; the cationic collector is selected from at least one of dodecylamine, octadecylamine, and etheramine. As a preferred embodiment, the present invention provides a process for comprehensive recovery of high-quality products from tailings; the anionic-cationic complex collector is composed of anionic collector and cationic collector in a mass ratio of anionic collector: cationic collector = 3:1-5:1.

[0013] As a preferred solution, the present invention provides a process for comprehensively recovering high-quality products from tailings; after separating the mica, a quartz activator and an anion collector are added to carry out quartz flotation; the quartz activator is calcium ions.

[0014] As a preferred solution, the present invention provides a process for comprehensively recovering high-quality products from tailings; the tailings include tungsten tailings, preferably re-selected tungsten tailings and / or tungsten flotation tailings.

[0015] As a preferred solution, the present invention provides a process for comprehensively recovering high-quality products from tailings, comprising the following steps:

[0016] The first step is to add sodium carbonate to the tailings according to the standard of adding 1000-1500g sodium carbonate per ton of tailings for grinding, so that the fineness of the grinding product reaches -0.074mm and the content is 65-75%, and the ground tailings are mixed with water to form a 30%-40% slurry;

[0017] The second step is to stir for 8-10 minutes, settle for 5-7 minutes and then siphon desludging;

[0018] The third step is to add sodium carbonate to adjust the pH value of the slurry to 10.00-10.60, add 300-400g / t of anion-cation complex collector per ton of tailings to float and separate mica from the tailings, continue to adjust the slurry to 10.00-10.60, and reduce the dosage of the reagent by half to sweep the first stage;

[0019] The fourth step is to add sodium carbonate to adjust the pH value of the pulp to 10.60-11.00, add 150-250g of Ca ions and 300-500g of anion collector per ton of tailings to float and separate the quartz in the tailings, continue to adjust the pulp to 10.60-11.00, and reduce the dosage of reagents by half to scavenging; after scavenging and / or flotation of quartz, the material remaining at the bottom of the tank is mainly feldspar, and the feldspar is subjected to high gradient iron removal, the magnetic field strength is 1.5-1.8T, and the non-magnetic product is high-quality feldspar;

[0020] The fifth step is to adjust the foam product (i.e., quartz product) to adjust the pH of the slurry to 10.60-11.00, the slurry concentration to 25-35%, and perform two concentrations without adding chemicals. The tailings of each concentration operation are returned to the previous operation in sequence;

[0021] In the sixth step, the foam product (i.e., quartz product) that has been selected twice is re-slurried, the pH value of the slurry is adjusted to 2.70-3.20, the slurry concentration is 25-35%, 60-80g of cationic collector is added per ton of tailings, and quartz is removed by aeration. The slurry is continued to be adjusted to 2.70-3.20, and the dosage of the reagent is halved to sweep the first selection; after two flotation removals, the main material remaining at the bottom of the tank is high-quality quartz.

[0022] As a preferred solution, the present invention provides a process for comprehensively recovering high-quality products from tailings; the silicon dioxide content in the obtained quartz product is greater than or equal to 99.2%; the potassium oxide and sodium oxide contents in the obtained high-quality feldspar product will change with the properties of the original ore, but both meet the first-class product standards.

[0023] As a preferred solution, the present invention provides a process for comprehensively recovering high-quality products from tailings; the yield of quartz products is greater than or equal to 34%, preferably 34-38.5%.

[0024] As a preferred solution, the invention provides a process for comprehensively recovering high-quality products from tailings; the yield of feldspar products is greater than or equal to 24.5%, preferably 24.8-31.6%. In the preferred solution of the invention, the output of quartz products and the output of feldspar products are both greater than 24.8%.

[0025] Compared with the prior art, the advantages of the present invention are:

[0026] (1) The process of the present invention is carried out under fluorine-free and acid-free slurry conditions, which can avoid the corrosion of mineral processing equipment and pipelines under acidic conditions, and also avoid the harm of fluoride ions to the environment and human body caused by the hydrofluoric acid solution.

[0027] (2) There are a large number of non-metallic mineral resources in my country's tailings. Due to the constraints of mineral processing technology and economic benefits, a huge waste of resources has been caused. The process of the present invention can better recover mica, quartz and feldspar in tungsten tailings, and has great promotion value.

[0028] (3) The process of the present invention not only recycles a large amount of non-metallic mineral resources, but also can greatly reduce the discharge of mine tailings, and even make all mine tailings recyclable, thus realizing tailing-free mines.

[0029] (4) The quartz product obtained by the process of the present invention is adjusted to a weakly acidic slurry with a concentration of 25-30% and a pH value of 2.7-3.2, and 50-100g of the cationic collector per ton of tailings of the present invention is added, and aeration flotation is performed to purify the silicon dioxide in the quartz product to greater than or equal to 99.2%. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 XRD pattern of the raw materials used in Example 1;

[0031] Figure 2 XRD pattern of the raw materials used in Example 3;

[0032] Figure 3 To explore the mica flotation phenomenon diagram under different pulp pH conditions in case series 1, a is the mica flotation phenomenon and mica product phase diagram when pH is 9.80, b is the mica flotation phenomenon and mica product phase diagram when pH is 10.35, and c is the mica flotation phenomenon and mica product phase diagram when pH is 10.80;

[0033] Figure 4 This is a graph comparing the mica flotation concentrate yield under different anion and cation collector ratios in case series 2;

[0034] Figure 5 It is a process flow chart of the present invention. DETAILED DESCRIPTION

[0035] The technical solution of the present invention is further described in detail below through specific implementation methods.

[0036] Example 1 and Comparative Examples 1, 2, 3, and 4

[0037] This embodiment and comparative examples 1, 2, 3, and 4 all use the gravity separation tailings of a tungsten mine in Ninghua, Fujian as raw materials. The main phase analysis of the gravity separation tailings of the tungsten is shown in FIG. Figure 1 The contents of the main substances are shown in Table 1. This embodiment uses the process technology provided by the present invention to separate mica, quartz and feldspar from the gravity-selected tailings of tungsten in Ninghua, Fujian, so that the feldspar product reaches the first-class product and the quartz product reaches the sales standard. The mineral composition of the gravity-selected tailings is mainly quartz, feldspar, mica and some impurities with a smaller content. The tailings fineness -0.074mm accounts for 12.73%, the relative content of mica minerals is about 14%, the relative content of quartz minerals is about 48%, and the relative content of feldspar minerals is about 33%. The content of the three minerals in the gravity-selected tailings is about 95%.

[0038] The present embodiment provides a flotation separation process for flotation separation of mica and quartz feldspar from tailings, which specifically includes the following steps:

[0039] Pretreatment (grinding, desliming): weigh 500g of the gravity separation tailings, and grind them according to the standard of adding 1200g of sodium carbonate per ton of tailings. In Example 1, Comparative Example 3 and Comparative Example 4, the gravity separation tailings are ground to a fineness of -0.074mm and a content of about 70%. In Comparative Example 1 and Comparative Example 2, the gravity separation tailings are ground to a fineness of -0.074mm and a content of about 57% and 81%, respectively. The ground product is placed in a 1.5L flotation machine, and the fine mud in the slurry is removed by sedimentation siphon to obtain mica, quartz, and feldspar products to be flotation separated.

[0040] Mica flotation: The pre-treated sample (i.e., the mica, quartz, and feldspar products to be separated by flotation obtained in the previous step) is first subjected to mica flotation. The mica flotation process of the embodiment and the comparative example is the same. Sodium carbonate is added to adjust the pH value of the slurry to 10.47, the ratio (mass ratio) of the anion and cation associated collectors is fixed to 4:1 (wherein the anion collector is sodium oleate; the cationic collector is dodecylamine), the total amount of mica roughing agent is 400g / t, the slurry is continued to be adjusted to 10.47, and the amount of the agent is halved for one sweep. The yields of the foam products (i.e., mica products) of Example 1, Comparative Example 1, Comparative Example 2, Comparative Example 3, and Comparative Example 4 are 12.23%, 10.14%, 13.72%, 11.98%, and 12.11%, respectively, and the bottom product is subjected to quartz and feldspar flotation separation.

[0041] Quartz flotation: Example 1, Comparative Example 1 and Comparative Example 2 add sodium carbonate to adjust the pH value of the ore pulp to 10.70, Comparative Example 3 and Comparative Example 4 add sodium carbonate to adjust the pH value of the ore pulp to 10.00 and 11.50, respectively, and add 200g Ca ions and 400g anion collector-sodium oleate per ton of tailings to flotation and separate quartz in the tailings; Continue to add sodium carbonate to adjust the pH value of the ore pulp to 10.70 in Example 1, Comparative Example 1 and Comparative Example 2, and add sodium carbonate to adjust the pH value of the ore pulp to 10.00 and 11.50 in Comparative Example 3 and Comparative Example 4, respectively, and reduce the dosage of the reagent by half to sweep one, and the bottom of the flotation tank is a feldspar product, which is subjected to strong magnetic iron removal, and the non-magnetic product is filtered and dried for testing.

[0042] Quartz selection: Quartz products are mainly enriched in flotation foam. The foam product of quartz flotation is slurried, and the concentration of the first quartz selection is 33%. In Example 1, Comparative Example 1 and Comparative Example 2, sodium carbonate is added to adjust the pH value of the slurry to 10.70. In Comparative Example 3 and Comparative Example 4, sodium carbonate is added to adjust the pH value of the slurry to 10.00 and 11.50 respectively. No chemicals are added to select one time, and the bottom of the flotation tank is medium ore, which is returned to the quartz scavenging operation; the foam of the first quartz selection is continued to be slurried, and the concentration of the second quartz selection is 27%. In Example 1, Comparative Example 1 and Comparative Example 2, sodium carbonate is added to adjust the pH value of the slurry to 10.70. In Comparative Example 3 and Comparative Example 4, sodium carbonate is added to adjust the pH value of the slurry to 10.00 and 11.50 respectively. No chemicals are added to select one time, and the bottom of the flotation tank is medium ore, which is returned to the first quartz selection operation;

[0043] Quartz weak acid impurity removal: The foam products selected twice in the examples and comparative examples were slurried, the slurry concentration was 26%, the slurry pH was 2.80, 60g of cationic collector dodecylamine was added per ton of tailings, and the quartz impurities were removed by aeration. The slurry was continued to be adjusted to 2.80, and the dosage of the reagent was halved to sweep the first selection; after two flotation impurities removal, the main residue at the bottom of the tank was high-quality quartz.

[0044] Table 1. Comparison of the properties of the gravity separation tailings of a tungsten mine in Ninghua, Fujian, with feldspar and quartz products

[0045]

[0046] By comparison with Example 1, it can be seen that when the grinding fineness is coarse and the slurry pH value is low, quartz floats incompletely and the feldspar product index is low; when the grinding fineness is fine, the quartz product and feldspar product indexes are normal, but the yields of the two products are low; when the slurry pH value is high, feldspar floats into the foam product, and the quartz product and feldspar product indexes are both low.

[0047] Example 2 and Comparative Example 5

[0048] This embodiment and comparative example are both based on the gravity separation tailings of a tungsten mine in Ninghua, Fujian as raw materials (basically the same composition as the raw materials in Example 1). The main phase analysis of the gravity separation tailings of tungsten is shown in Figure 1 The contents of the main substances are shown in Table 2. This embodiment uses the process technology provided by the present invention to separate mica, quartz and feldspar from the gravity separation tailings of tungsten in Ninghua, Fujian, so that the feldspar product reaches the first-class product and the quartz product reaches the sales standard.

[0049] The mineral composition of the gravity separation tailings is mainly quartz, feldspar, mica and some impurities with less content. The tailings fineness is -0.074mm, accounting for 12.73%, the relative content of mica minerals is about 18%, the relative content of quartz minerals is about 47%, and the relative content of feldspar minerals is about 32%. The content of these three minerals in the gravity separation tailings exceeds 95%.

[0050] The present embodiment provides a flotation separation process for flotation separation of mica and quartz feldspar from tailings, which specifically includes the following steps:

[0051] Pre-treatment (grinding, desliming): weigh 500g of the gravity separation tailings, grind them according to the standard of adding 1300g of sodium carbonate per ton of tailings, grind the gravity separation tailings to a fineness of -0.074mm and a content of 72.4%, put the ground product of Example 2 into a 1.5L flotation machine, and remove the fine mud in the slurry by sedimentation siphoning. The ground product of Comparative Example 5 is not deslimed (the subsequent treatment is consistent with Example 2), and two groups of mica, quartz and feldspar products to be flotation separated are obtained.

[0052] Mica flotation: The pre-treated sample was first subjected to mica flotation. The pH value of sodium carbonate pulp flotation was 10.53, and the ratio (mass ratio) of anionic and cationic associating collectors was fixed at 3:1 (wherein the anionic collector was oxidized paraffin soap; the cationic collector was octadecylamine). The total amount of mica roughing agent was 360 g / t. The pulp was continued to be adjusted to 10.53, and the amount of agent was halved for sweeping. The yields of the foam products (i.e., mica products) of Example 2 and Comparative Example 5 were 12.13% and 12.31%, respectively. The bottom product of the tank was subjected to quartz and feldspar flotation separation.

[0053] Quartz flotation: add sodium carbonate to adjust the pH value of the pulp to 10.80, add 220g Ca ions and 440g anion collector-oxidized paraffin soap per ton of tailings, and then float to separate the quartz in the tailings; continue to adjust the pulp to 10.80, reduce the amount of reagents by half, and sweep the first step. The bottom of the flotation tank is the feldspar product. After strong magnetic iron removal, it is filtered and dried for testing.

[0054] Quartz selection: Quartz products are mainly enriched in flotation foam. The foam product of quartz flotation is pulped, and the pH value of the pulp is adjusted to 10.80. The first selection is carried out without adding chemicals. The bottom of the flotation tank is medium ore, which is returned to the quartz scavenging operation after concentration. The foam of the first selection of quartz is continued to be pulped, and the pH value of the pulp is adjusted to 10.80. The first selection is carried out without adding chemicals. The bottom of the flotation tank is medium ore, which is returned to the first selection of quartz after concentration.

[0055] Quartz weak acid impurity removal: The foam products selected twice in Example and Comparative Example 5 were slurried, the pulp concentration was 30%, the pulp pH was 2.85, 80g of cationic collector octadecylamine was added per ton of tailings, and the quartz impurities were removed by aeration. The pulp was continued to be adjusted to 2.85, and the dosage of the reagent was halved to select one stage; after two flotation impurities removal, the main material remaining at the bottom of the tank was high-quality quartz.

[0056] Table 2. Comparison of the properties of the gravity separation tailings of a tungsten mine in Ninghua, Fujian, and the feldspar and quartz products

[0057]

[0058] By comparing Comparative Example 5 with Example 2, it can be seen that when the ore sample is not deslimed and mica and quartz are directly flotated, flotation is basically impossible due to the high content of fine particles in the slurry.

[0059] Example 3 and Comparative Example 6

[0060] This embodiment and comparative example 6 both use flotation tailings of a tungsten mine in a certain area of ​​Jiangxi as raw materials. The main phase analysis of the flotation tailings of tungsten is shown in FIG. Figure 2 The contents of the main substances are shown in Table 3. This embodiment uses the process technology provided by the present invention to separate mica, quartz and feldspar from the re-selection tailings of tungsten in a certain area of ​​Jiangxi Province, so that the feldspar product reaches the first-class product and the quartz product reaches the sales standard.

[0061] The mineral composition of the flotation tailings is mainly quartz, feldspar, mica and some impurities with less content such as chlorite. The tailings fineness is -0.074mm, accounting for 30.13%, the relative content of mica minerals is about 16%, the relative content of quartz minerals is about 38%, and the relative content of feldspar minerals is about 37%. The content of these three minerals in the flotation tailings exceeds 93%.

[0062] The present embodiment provides a flotation separation process for flotation separation of mica and quartz feldspar from tailings, which specifically includes the following steps. The pre-treatment, mica flotation, quartz flotation and quartz concentration processes of Example 3 and Comparative Example 6 are the same:

[0063] Pre-treatment (grinding, desliming): weigh 500g of the flotation tailings, grind them according to the standard of adding 1300g of sodium carbonate per ton of tailings, grind the gravity separation tailings to a fineness of -0.074mm and a content of 68.45%, put the ground product into a 1.5L flotation machine, and remove the fine mud in the slurry by sedimentation siphon to obtain mica, quartz and feldspar flotation separation products.

[0064] Mica flotation: The pre-treated sample was first subjected to mica flotation. The pH value of sodium carbonate pulp flotation was 10.20, the ratio (mass ratio) of anionic and cationic associating collectors was fixed to 5:1 (wherein the anionic collector was tall oil; the cationic collector was etheramine), the total amount of mica roughing agent was 360 g / t, the pulp was continued to be adjusted to 10.20, the amount of agent was halved for sweeping, the yields of the foam products (i.e., mica products) of Example 3 and Comparative Example 6 were 12.32% and 12.08%, respectively, and the bottom product of the tank was subjected to quartz and feldspar flotation separation.

[0065] Quartz flotation: add sodium carbonate to adjust the pH value of the pulp to 10.64, add 180g Ca ions and 360g anion collector-tall oil per ton of tailings, and then float to separate the quartz in the tailings; continue to adjust the pulp to 10.64, reduce the amount of reagents by half, and sweep the first step. The bottom of the flotation tank is the feldspar product. After strong magnetic iron removal, it is filtered and dried for testing.

[0066] Quartz selection: Quartz products are mainly concentrated in flotation foam. The foam product of quartz flotation is pulped, and the pH value of the pulp is adjusted to 10.64. No chemicals are added to the first selection. The bottom of the flotation tank is the medium ore. After concentration, it returns to the quartz scavenging operation; continue to pulp the foam of the first selection of quartz, and adjust the pH value of the pulp to 10.64 at the same time. No chemicals are added to select again. The bottom of the flotation tank is the medium ore. After concentration, it returns to the first selection of quartz. (If it is used as a comparative example, it will get the product by doing this step)

[0067] Quartz weak acid impurity removal: The foam product selected twice in Example 3 was slurried, the pulp concentration was 30%, the pulp pH was 2.85, 80g of cationic collector etheramine was added per ton of tailings, and the quartz was aerated for impurity removal. The pulp was continued to be adjusted to 2.85, and the dosage of the reagent was halved to sweep the first selection; after two flotation impurities removal, the main residue at the bottom of the tank was high-quality quartz; the foam product of quartz selected twice in Comparative Example 6 was not treated by the weak acid impurity removal process.

[0068] Table 3. Comparison of the flotation tailings properties of a tungsten mine in a certain area of ​​Jiangxi with feldspar and quartz products

[0069]

[0070] It can be seen from Example 6 compared with Example 3 that the quartz mineral concentrate foam product is not treated with weak acid, and the silicon dioxide content in the quartz product is unqualified.

[0071] Explore Series Case 1

[0072] Comparative test of pH value of mica flotation pulp

[0073] This series of exploration cases uses the gravity separation tailings of a tungsten mine in Ninghua, Fujian as raw material (basically the same as the raw material in Example 1). The main phase analysis of the gravity separation tailings of the tungsten is shown in Figure 1 This embodiment uses the process technology provided by the present invention to separate mica from the gravity separation tailings of tungsten in Ninghua, Fujian.

[0074] The mineral composition of the gravity separation tailings is mainly quartz, feldspar, mica and some impurities with less content. The tailings fineness is -0.074mm, accounting for 12.73%, the relative content of mica minerals is about 18%, the relative content of quartz minerals is about 47%, and the relative content of feldspar minerals is about 28%. The content of these three minerals in the gravity separation tailings exceeds 95%.

[0075] The flotation separation process of mica from tailings provided in this exploration series case includes the following steps:

[0076] Pre-treatment (grinding, desliming): weigh 500g of the gravity separation tailings, grind them according to the standard of adding 1300g of sodium carbonate per ton of tailings, grind the gravity separation tailings to a fineness of -0.074mm and a content of 72.4%, put the ground product into a 1.5L flotation machine, and remove the fine mud in the slurry by sedimentation siphon to obtain mica, quartz and feldspar flotation separation products.

[0077] Mica flotation: The pre-treated samples were first subjected to mica flotation. The ratio (mass ratio) of anion and cation associated collectors was fixed at 5:1 (among which the anion collector was sodium oleate and the cationic collector was dodecylamine). The total dosage of mica roughing agent was 360g / t. The pH value of the pulp was adjusted to different values. The flotation phenomenon was as follows: Figure 3 shown. Figure 3 a is the mica flotation phenomenon and phase diagram of mica products when the pulp pH is 9.80. The mica flotation foam is relatively weak, and the mica product is entrained with more feldspar; Figure 3 b is the mica flotation phenomenon and the phase diagram of mica products when the pulp pH is 10.35. The mica flotation foam is relatively solid, and there is basically no feldspar entrained in the mica product; Figure 3 c is the mica flotation phenomenon and mica product phase diagram when the pulp pH is 10.80. The mica flotation foam is relatively solid, but the mica product contains more feldspar. Therefore, the flotation pH value is not easy to be too low or too alkaline, so the pulp pH value range for mica flotation is 10.00-10.60.

[0078] Explore Case 2

[0079] Comparative test on the ratio of collectors for anionic and cationic complexes in mica flotation

[0080] This embodiment uses the gravity separation tailings of a tungsten mine in Ninghua, Fujian as raw material (basically the same as the raw material in Example 1). The main phase analysis of the gravity separation tailings of tungsten is as follows: Figure 1 This embodiment uses the process technology provided by the present invention to separate mica from the gravity separation tailings of tungsten in Ninghua, Fujian.

[0081] The mineral composition of the gravity separation tailings is mainly quartz, feldspar, mica and some impurities with less content. The tailings fineness is -0.074mm, accounting for 12.73%, the relative content of mica minerals is about 18%, the relative content of quartz minerals is about 47%, and the relative content of feldspar minerals is about 28%. The content of these three minerals in the gravity separation tailings exceeds 95%.

[0082] The flotation separation process of mica from tailings provided in this exploration series case includes the following steps:

[0083] Pre-treatment (grinding, desliming): weigh 500g of the gravity separation tailings, grind them according to the standard of adding 1300g of sodium carbonate per ton of tailings, grind the gravity separation tailings to a fineness of -0.074mm and a content of 72.4%, put the ground product into a 1.5L flotation machine, and remove the fine mud in the slurry by sedimentation siphon to obtain mica, quartz and feldspar flotation separation products.

[0084] Mica flotation: The pre-treated samples were first subjected to mica flotation. The pH value of sodium carbonate pulp flotation was 10.40. The total amount of anion-cation associating collector was fixed at 360 g / t. The ratio of anions and cations was adjusted (the anion collector was sodium oleate and the cationic collector was dodecylamine). The mica flotation yield was as follows: Figure 4 As shown in the figure, the two collector ratios have a great influence on mica flotation. As the ratio of anionic collector to cationic collector increases, the yield of mica flotation concentrate decreases. When the ratio of collector TB-1:TB-2 is in the range of 3:1 to 5:1, the yield of mica flotation concentrate remains unchanged. When the ratio is below this range, the yield of mica flotation concentrate begins to decrease.

[0085] Comparative Example 7

[0086] Comparative test of quartz flotation activator with less dosage

[0087] This embodiment uses the gravity separation tailings of a tungsten mine in Ninghua, Fujian as raw material (basically the same as the raw material in Example 1). The main phase analysis of the gravity separation tailings of tungsten is as follows: Figure 1The contents of the main substances are shown in Table 4. This embodiment uses the process technology provided by the present invention to separate mica from the gravity separation tailings of tungsten in Ninghua, Fujian.

[0088] The mineral composition of the gravity separation tailings is mainly quartz, feldspar, mica and some impurities with less content. The tailings fineness is -0.074mm, accounting for 12.73%, the relative content of mica minerals is about 18%, the relative content of quartz minerals is about 47%, and the relative content of feldspar minerals is about 28%. The content of these three minerals in the gravity separation tailings exceeds 95%.

[0089] The present embodiment provides a flotation separation process for flotation separation of mica from tailings, which specifically includes the following steps:

[0090] Pre-treatment (grinding, desliming): weigh 500g of the gravity separation tailings, grind them according to the standard of adding 1300g of sodium carbonate per ton of tailings, grind the gravity separation tailings to a fineness of -0.074mm and a content of 72.4%, put the ground product into a 1.5L flotation machine, and remove the fine mud in the slurry by sedimentation siphon to obtain mica, quartz and feldspar flotation separation products.

[0091] Mica flotation: The pre-treated sample was first subjected to mica flotation. The pH value of sodium carbonate pulp flotation was 10.47, the ratio (mass ratio) of anion and cation associated collectors was fixed at 4:1 (the anion collector was sodium oleate; the cationic collector was dodecylamine), the total amount of mica roughing agent was 400g / t, the pulp was continued to be adjusted to 10.47, the amount of agent was halved, and the yield of the foam product (i.e., mica product) of Comparative Example 7 was 12.11%, and the bottom product of the tank was subjected to quartz and feldspar flotation separation.

[0092] Quartz flotation: add sodium carbonate to adjust the pH value of the pulp to 10.70, add 80g Ca ions and 400g anion collector per ton of tailings to float and separate the quartz in the tailings; continue to adjust the pulp to 10.70, reduce the amount of reagents by half, and sweep the first step. The bottom of the flotation tank is the feldspar product. After strong magnetic iron removal, it is filtered and dried for testing.

[0093] Quartz selection: Quartz products are mainly enriched in flotation foam. The foam product of quartz flotation is pulped, and the pH value of the pulp is adjusted to 10.70. The first selection is carried out without adding chemicals. The bottom of the flotation tank is the medium ore, which is returned to the tank after roughing in quartz flotation after concentration. The foam of the first selection of quartz is pulped, and the pH value of the pulp is adjusted to 10.70. The first selection is carried out without adding chemicals. The bottom of the flotation tank is the medium ore, which is returned to the tank before the first selection of quartz after concentration.

[0094] Quartz weak acid impurity removal: the foam product after two flotation separations is slurried to a pulp concentration of 26% and a pulp pH of 2.80. 60g of cationic collector dodecylamine is added per ton of tailings, and the quartz impurities are removed by aeration. The pulp is then adjusted to 2.80 and the dosage of reagents is halved to remove impurities in the first flotation separation. After two flotation separations, the main material remaining at the bottom of the tank is high-quality quartz.

[0095] Table 4. Comparison of the properties of the gravity separation tailings of a tungsten mine in Ninghua, Fujian, and the feldspar and quartz products

[0096]

[0097] In this comparative example (compared with Example 1), the quartz yield is too low; the obtained feldspar product is not pure enough and contains too many impurities.

[0098] Comparative Example 8

[0099] Comparative test of quartz flotation activator with high dosage

[0100] This embodiment uses the gravity separation tailings of a tungsten mine in Ninghua, Fujian as raw material (basically the same as the raw material composition of Example 3). The main phase analysis of the gravity separation tailings of tungsten is shown as follows: Figure 1 The contents of the main substances are shown in Table 5. This embodiment uses the process technology provided by the present invention to separate mica from the gravity separation tailings of tungsten in Ninghua, Fujian.

[0101] The mineral composition of the gravity separation tailings is mainly quartz, feldspar, mica and some impurities with less content. The tailings fineness is -0.074mm, accounting for 12.73%, the relative content of mica minerals is about 18%, the relative content of quartz minerals is about 47%, and the relative content of feldspar minerals is about 28%. The content of these three minerals in the gravity separation tailings exceeds 95%.

[0102] Mica flotation: The pre-treated sample was first subjected to mica flotation. The pH value of sodium carbonate pulp flotation was 10.47, the ratio (mass ratio) of anion and cation associated collectors was fixed at 4:1 (the anion collector was sodium oleate; the cationic collector was dodecylamine), the total amount of mica roughing agent was 400g / t, the pulp was continued to be adjusted to 10.47, the amount of agent was halved, and the yield of the foam product (i.e., mica product) of Comparative Example 8 was 12.34%, and the bottom product of the tank was subjected to quartz and feldspar flotation separation.

[0103] Quartz flotation: add sodium carbonate to adjust the pH value of the pulp to 10.70, add 300g Ca ions and 400g anion collector per ton of tailings to float and separate the quartz in the tailings; continue to adjust the pulp to 10.70, reduce the amount of reagents by half, and sweep the first step. The feldspar product is at the bottom of the flotation tank. After strong magnetic iron removal, it is filtered and dried for testing.

[0104] Quartz selection: Quartz products are mainly enriched in flotation foam. The foam product of quartz flotation is pulped, and the pH value of the pulp is adjusted to 10.70. The first selection is carried out without adding chemicals. The bottom of the flotation tank is the medium ore, which is returned to the tank after roughing in quartz flotation after concentration. The foam of the first selection of quartz is pulped, and the pH value of the pulp is adjusted to 10.70. The first selection is carried out without adding chemicals. The bottom of the flotation tank is the medium ore, which is returned to the tank before the first selection of quartz after concentration.

[0105] Quartz weak acid impurity removal: the foam product after two flotation separations is slurried to a pulp concentration of 26% and a pulp pH of 2.80. 60g of cationic collector dodecylamine is added per ton of tailings, and the quartz impurities are removed by aeration. The pulp is then adjusted to 2.80 and the dosage of reagents is halved to remove impurities in the first flotation separation. After two flotation separations, the main product remaining at the bottom of the tank is quartz.

[0106] Table 5. Comparison of the properties of the gravity separation tailings of a tungsten mine in Ninghua, Fujian, with feldspar and quartz products

[0107]

[0108] In this comparative example (compared with Example 1), there are too many impurities in the quartz product; the yield of the obtained feldspar product is too low.

Claims

1. A process for comprehensive recovery of high-quality products from tailings, characterized by: The tailings are ground and then separated by flotation at a pH of 10.00-10.60 for mica separation, followed by flotation separation of quartz at a pH of 10.60-11.

00. After the quartz flotation, the residue at the bottom of the tank is the feldspar product. The quartz is then separated twice as a foam product at a pH of 10.60-11.00, followed by acid separation of the quartz at a pH of 2.70-3.20 to remove impurities, ultimately yielding high-quality feldspar and quartz products. The collector used in the mica flotation separation is an anionic-cationic complex collector. The activator used in the quartz flotation separation is a metal ion activator, the collector is an anionic collector, and the collector used in the quartz acid separation is a cationic collector. The anionic collectors are all fatty acid collectors; the cationic collectors are all amine collectors; The activator for the quartz flotation separation is calcium ions.

2. The process for comprehensive recovery of high-quality products from tailings according to claim 1, characterized in that: The anionic collector is selected from at least one of oleic acid, oxidized paraffin soap, and tall oil; and the cationic collector is selected from at least one of dodecylamine, octadecylamine, and etheramine.

3. The process for comprehensive recovery of high-quality products from tailings according to claim 1, characterized in that: The anion-cation complex collector for mica flotation is composed of an anion collector and a cationic collector in a mass ratio; wherein the mass ratio of anion collector to cationic collector is 3:1-5:

1.

4. The process for comprehensive recovery of high-quality products from tailings according to claim 1, characterized in that: The activator for the quartz flotation separation is calcium chloride reagent.

5. The process for comprehensive recovery of high-quality products from tailings according to claim 1, characterized in that: The tailings are selected from at least one of tungsten tailings, molybdenum tailings and kaolin tailings.

6. A process for comprehensive recovery of high-quality products from tailings according to any one of claims 1 to 5, characterized in that: The steps include: The first step is to add sodium carbonate to the tailings according to the standard of adding 1000-1500g sodium carbonate per ton of tailings for grinding, so that the fineness of the grinding product reaches -0.074mm and the content is 65-75%. The ground tailings are mixed with water to form a 30%-40% slurry; The second step is to stir for 8-10 minutes, settle for 5-7 minutes and then siphon desludging; The third step is to add sodium carbonate to adjust the pH value of the slurry to 10.00-10.60, add 300-400g / t of anion-cation complex collector per ton of tailings to float and separate mica from the tailings, continue to adjust the slurry to 10.00-10.60, and reduce the amount of reagent by half to sweep the first stage; In the fourth step, sodium carbonate is added to adjust the pH value of the slurry to 10.60-11.

00. 150-250g of Ca ions and 300-500g of anionic collector are added per ton of tailings to flotate and separate the quartz in the tailings. The slurry is then adjusted to 10.60-11.00 and the reagent dosage is halved to perform a scavenging step. After scavenging and / or flotation of quartz, the material remaining at the bottom of the tank is mainly feldspar. The feldspar is subjected to high-gradient iron removal with a magnetic field strength of 1.5-1.8T. The non-magnetic product is high-quality feldspar. The fifth step is to adjust the foam product to a slurry pH of 10.60-11.00 and a slurry concentration of 25-35%. The slurry is then beneficiated twice without adding chemicals. The tailings from each beneficiation operation are returned to the previous operation in sequence. In the sixth step, the foam product that has been selected twice is re-slurried, the pulp pH is adjusted to 2.70-3.20, the pulp concentration is 25-35%, 60-80g of cationic collector is added per ton of tailings, and quartz is removed by aeration. The pulp is continued to be adjusted to 2.70-3.20, and the amount of reagents is halved to sweep the first selection; after two flotation separations, the main residue at the bottom of the tank is high-quality quartz.

7. A process for comprehensive recovery of high-quality products from tailings according to any one of claims 1 to 5, characterized in that: The silicon dioxide content in the obtained high-quality quartz product is greater than or equal to 99.2%; the potassium oxide and sodium oxide contents in the obtained high-quality feldspar product will vary with the properties of the original ore, but both meet the first-class product standards.

8. A process for comprehensive recovery of high-quality products from tailings according to any one of claims 1 to 5, characterized in that: The output rates of quartz products and feldspar products are both greater than 24.5%.

9. A process for comprehensive recovery of high-quality products from tailings according to any one of claims 1 to 5, characterized in that: The yield of quartz products is greater than or equal to 34%; the yield of feldspar products is greater than or equal to 24.5%.

10. The process for comprehensive recovery of high-quality products from tailings according to claim 9, characterized in that: The yield of quartz products is 34-38.5%; the yield of feldspar products is 24.8-31.6%.

Citation Information

Patent Citations

  • Method for recovering feldspar from molybdenum separation tailings

    CN103447146A

  • Method for recovering potash feldspar and quartz from gold tailings

    CN110142133A

  • Method for recovering mica and feldspar quartz from rare metal beneficiation tailings

    CN111389598A

  • Comprehensive recovery process of low-grade fine-grained niobium-tantalum ore

    CN112452532A

  • Flotation process for separating silica from feldspar to form a feed material for making glass

    US6098810A