A three-dimensional porous metal-free electrode, preparation method and application thereof
By preparing a three-dimensional porous metal-free electrode, using freeze-drying and pyrolysis treatment of melamine foam, combined with the doping of nitrogen- and boron-containing compounds, the problems of limited reactivity distribution and complex preparation of electro-Fenton electrode materials have been solved, and high efficiency has been achieved. Degradation of organic pollutants and environmentally friendly electro-Fenton catalysis effect.
Patent Information
- Application Number
- CN202211389846.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-08
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-11-08
AI Technical Summary
Existing electro-Fenton electrode materials have limited reactive phase distribution, limited mass transfer and diffusion, and cumbersome preparation methods, resulting in limited applications in the environmental field.
Three-dimensional porous metal-free electrodes are prepared using melamine foam through precursor solution impregnation, freeze-drying and pyrolysis. By regulating the molar ratio and doping of nitrogen- and boron-containing compounds, the charge distribution and pore structure are optimized to improve the degradation efficiency of organic pollutants. .
It achieves efficient degradation of organic pollutants, strengthens the mass transfer process, demonstrates an environmentally friendly reaction system, and the charge distribution can be controlled, improving the electro-Fenton catalytic activity and stability.
Smart Images

Figure HDA0003931553870000011 
Figure HDA0003931553870000012 
Figure HDA0003931553870000013
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electrocatalytic remediation of environmental pollution, and in particular to a three-dimensional porous metal-free electrode, a preparation method and application thereof. Background Art
[0002] Highly toxic and difficult-to-degrade organic pollutants discharged into water bodies have various adverse effects on the ecological environment and human life. At present, the use of advanced oxidation technology to degrade organic pollutants in water bodies has become a hot topic of widespread concern and is of great significance for solving the problem of environmental water pollution in my country. Among them, electro-Fenton degradation of organic wastewater stands out among many technologies because of its safety, easy operation, green and high efficiency.
[0003] Electro-Fenton can produce H2O2 in situ through a two-electron oxygen reduction reaction (2e-ORR) at the cathode. Through the active sites, the catalytic reaction of H2O2 obtains rich active free radicals for efficient mineralization and removal of organic pollutants. For electro-Fenton technology, how to effectively anchor the solid-phase reaction active sites on electrodes that are simple to operate and easy to recycle to achieve an efficient catalytic reaction process is a core issue in the preparation of electro-Fenton electrode materials. At the same time, environmentally friendly preparation routes and cost control are also key factors in meeting actual environmental application needs and the green development of the economy and society.
[0004] At present, the main types of electrode electro-Fenton materials are as follows: (1) using polymer binders to coat nanocatalysts on the surface of conductive substrates to prepare electrodes; (2) catalytic active phases are grown in situ on the surface of conductive substrates to prepare self-supporting electrodes. However, the reactive phases of the above electrode materials are mostly anchored on the electrode surface, with limited distribution, and are affected by the physical and chemical properties of the substrate surface such as functional group characteristics, porosity and conductivity, and the mass transfer and diffusion process of the active sites is subject to certain restrictions. Based on the preparation of electrode materials supported by conductive substrates, Zhao et al. used resorcinol, formaldehyde, etc. as raw materials and utilized gel-sol, solvent exchange, pyrolysis and gas activation treatment to prepare bulk FeCuC aerogel electrodes with three-dimensional structures for electro-Fenton treatment of dye wastewater (Zhao H, Qian L, Guan X, et al. Continuous Bulk FeCuC Aerogel with Ultradispersed Metal Nanoparticles: An Efficient 3DHeterogeneous Electro-Fenton Cathode over a Wide Range of pH 3-9[J]. Environmental Science&Technology, 2016, 50(10): 5225-5233). Zhang et al. successfully prepared a monolithic Fe3O4 / gas diffusion electrode for electro-Fenton degradation of tetracycline by using the complex cross-linking reaction between Fe3O4 / AC and polytetrafluoroethylene emulsion, alcohols and other precursors during heating (Zhang Y, Gao M, Wang S, et al. Integrated electro-Fenton process enabled by a rotating Fe3O4 / gas diffusion cathode for simultaneous generation and activation of H2O2 [J]. Electrochimica Acta, 2017, 231: 694-704). The above-mentioned monolithic three-dimensional electrode material is free from the constraints of the conductive substrate, has low interfacial charge transfer resistance, high specific surface area and porous structure, and exhibits excellent electro-Fenton catalytic activity. However, the limitations of pore regulation in the electrode body phase, agglomeration and masking of active components, cumbersome preparation methods, loss of traditional metal active components and secondary pollution hinder its application in the environmental field. Summary of the invention
[0005] In view of this, the technical problem to be solved by the present invention is to provide a three-dimensional porous metal-free electrode, a preparation method and application thereof, wherein the three-dimensional porous metal-free electrode can improve the degradation efficiency of organic pollutants.
[0006] The present invention provides a three-dimensional porous metal-free electrode, which is prepared by impregnating melamine foam with a precursor solution, followed by freeze drying and pyrolysis;
[0007] The precursor solution includes a nitrogen-containing compound and a boron-containing compound;
[0008] The molar ratio of the nitrogen-containing compound to the boron-containing compound is 10-80:1.
[0009] Preferably, the nitrogen-containing compound comprises at least one of polyvinyl pyrrolidone, urea, aniline, tert-butylamine, melamine, dicyandiamide, ammonium chloride, ammonium carbonate and chitosan;
[0010] The boron-containing compound comprises at least one of boric acid, borax, boron trioxide, borane, sodium borohydride, triphenyl boroxine, triethyl borate and 3-aminophenylboronic acid.
[0011] Preferably, the solvent in the precursor solution is ultrapure water.
[0012] The present invention also provides a method for preparing the three-dimensional porous metal-free electrode as described above, comprising the following steps:
[0013] A) immersing the melamine foam in a precursor solution for a period of time; the precursor solution comprises a nitrogen-containing compound and a boron-containing compound;
[0014] B) pre-freezing the impregnated melamine foam and then freeze-drying it;
[0015] C) subjecting the freeze-dried melamine foam to pyrolysis treatment in an inert gas atmosphere to obtain a three-dimensional porous metal-free electrode.
[0016] Preferably, in step A), the immersion temperature is room temperature and the time is 10 to 20 minutes.
[0017] Preferably, in step B), the pre-freezing temperature is -78 to -82°C and the time is 6 to 10 hours;
[0018] The freeze-drying temperature is -70 to -50°C and the time is 55 to 65 hours.
[0019] Preferably, in step C), the inert gas is nitrogen.
[0020] Preferably, in step C), the temperature of the pyrolysis treatment is 850-950° C. and the time is 1.5-2.5 h;
[0021] The temperature of the freeze-dried melamine foam is raised to the pyrolysis treatment temperature in an inert gas atmosphere at a heating rate of 4 to 6°C / min.
[0022] The present invention also provides an application of the three-dimensional porous metal-free electrode described above or the three-dimensional porous metal-free electrode prepared by the preparation method described above as an electro-Fenton cathode in wastewater treatment.
[0023] The present invention provides a three-dimensional porous metal-free electrode, which is prepared by melamine foam impregnated with a precursor solution, followed by freeze drying and pyrolysis; the precursor solution includes a nitrogen-containing compound and a boron-containing compound; the molar ratio of the nitrogen-containing compound to the boron-containing compound is 10 to 80:1. Compared with the prior art, the electrode material prepared by the present invention can improve the degradation efficiency of organic pollutants by strengthening the mass transfer process and the charge distribution control strategy, and the metal-free electro-Fenton process reflects the environmentally friendly characteristics of its reaction system. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a SEM image of the initial melamine foam of Comparative Example 1 of the present invention;
[0025] Figure 2 is a SEM image of the CF electrode of Comparative Example 1 of the present invention;
[0026] Figure 3 This is a SEM image of the N / CF electrode of Comparative Example 2 of the present invention;
[0027] Figure 4 is a SEM image of the NB / CF electrode of Example 1 of the present invention;
[0028] Figure 5 This is the XPS graph of the NB / CF electrode of Example 1 of the present invention;
[0029] Figure 6 This is a SEM image of the NB / CF1 electrode of Comparative Example 3 of the present invention;
[0030] Figure 7 is a SEM image of the NB / CF2 electrode of Example 2 of the present invention;
[0031] Figure 8 is a SEM image of the NB / CF3 electrode of Example 3 of the present invention;
[0032] Fig. 9 This is a SEM image of the NB / CF4 electrode of Comparative Example 4 of the present invention;
[0033] Fig.10 XRD diagrams of electrodes prepared in Examples 1 to 3 and Comparative Examples 1 to 4 of the present invention;
[0034] Fig.11 The electro-Fenton catalytic performance diagram of the electrodes prepared in Examples 1 to 3 of the present invention and Comparative Examples 1 to 4;
[0035] Fig.12 This is the electro-Fenton stability performance diagram of the NB / CF electrode of Example 1 of the present invention. DETAILED DESCRIPTION
[0036] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0037] The present invention provides a three-dimensional porous metal-free electrode, characterized in that it is prepared by impregnating melamine foam with a precursor solution, followed by freeze drying and pyrolysis;
[0038] The precursor solution includes a nitrogen-containing compound and a boron-containing compound;
[0039] The molar ratio of the nitrogen-containing compound to the boron-containing compound is 10-80:1.
[0040] In certain embodiments of the present invention, the nitrogen-containing compound comprises at least one of polyvinylpyrrolidone (PVP), urea, aniline, tert-butylamine, melamine, dicyandiamide, ammonium chloride, ammonium carbonate and chitosan.
[0041] In certain embodiments of the present invention, the boron-containing compound includes at least one of boric acid, borax, boron trioxide, borane, sodium borohydride, triphenylboroxine, triethyl borate and 3-aminophenylboronic acid.
[0042] In certain embodiments of the present invention, the solvent in the precursor solution is ultrapure water.
[0043] In certain embodiments of the present invention, the precursor solution is prepared according to the following method:
[0044] The nitrogen-containing compound, the boron-containing compound and ultrapure water are mixed and dissolved by ultrasonication to obtain a homogeneous mixed solution, which is a precursor solution.
[0045] The molar ratio of the nitrogen-containing compound to the boron-containing compound is 10 to 80: 1. In certain embodiments of the present invention, the molar ratio of the nitrogen-containing compound to the boron-containing compound is 40: 1, 20: 1 or 60: 1.
[0046] In the present invention, the melamine foam is an electrode substrate.
[0047] In certain embodiments of the present invention, the melamine foam is commercially available or prepared according to methods known to those skilled in the art. The density of the melamine foam is 8 kg / m 3 The melamine foam can be cut according to the required size, and the size after cutting can be 5cm×2cm×1cm.
[0048] The three-dimensional porous metal-free electrode provided by the present invention has a porous structure, which can provide abundant anchoring space and enhance the mass transfer diffusion process. Heteroatom doping can regulate the surface charge distribution, and achieve efficient electro-Fenton degradation of organic matter by optimizing the chemical adsorption and desorption process of reaction molecules such as O2 and OOH*.
[0049] The present invention also provides a method for preparing the three-dimensional porous metal-free electrode as described above, comprising the following steps:
[0050] A) immersing the melamine foam in a precursor solution for a period of time; the precursor solution comprises a nitrogen-containing compound and a boron-containing compound;
[0051] B) pre-freezing the impregnated melamine foam and then freeze-drying it;
[0052] C) subjecting the freeze-dried melamine foam to pyrolysis treatment in an inert gas atmosphere to obtain a three-dimensional porous metal-free electrode.
[0053] The raw materials used in the preparation method of the three-dimensional porous metal-free electrode are the same as above and will not be described in detail here.
[0054] In step A):
[0055] The melamine foam is immersed in a precursor solution for a period of time; the precursor solution includes a nitrogen-containing compound and a boron-containing compound.
[0056] In certain embodiments of the present invention, the immersion temperature is room temperature, and the immersion time is 10 to 20 minutes; specifically, it can be 15 minutes.
[0057] In step B):
[0058] The impregnated melamine foam is pre-frozen and then freeze-dried.
[0059] In certain embodiments of the present invention, the pre-freezing temperature is -78 to -82°C, specifically, -80°C; the pre-freezing time is 6 to 10 hours, specifically, 8 hours.
[0060] In certain embodiments of the present invention, the freeze drying temperature is -70 to -50°C, and the time is 55 to 65 hours. Specifically, the freeze drying temperature is -60°C; the freeze drying time is 60 hours. The freeze drying is performed in a freeze dryer.
[0061] In step C):
[0062] The freeze-dried melamine foam is pyrolyzed in an inert gas atmosphere to obtain a three-dimensional porous metal-free electrode.
[0063] In certain embodiments of the present invention, the inert gas is nitrogen.
[0064] In certain embodiments of the present invention, the temperature of the pyrolysis treatment is 850-950° C., specifically, 900° C.; the time is 1.5-2.5 h, specifically, 2 h.
[0065] In certain embodiments of the present invention, the temperature rise rate of the freeze-dried melamine foam in an inert gas atmosphere to the pyrolysis treatment temperature is 4-6°C / min; specifically, it can be 5°C / min.
[0066] The present invention also provides an application of the three-dimensional porous metal-free electrode described above or the three-dimensional porous metal-free electrode prepared by the preparation method described above as an electro-Fenton cathode in wastewater treatment. The wastewater may be wastewater containing organic pollutants. The organic pollutant may be metronidazole.
[0067] Specifically, the wastewater treatment method includes:
[0068] The mixed solution of wastewater and sodium sulfate is used as an electrolyte, the three-dimensional porous metal-free electrode described above is used as a cathode, and the platinum sheet is used as an anode to treat the wastewater;
[0069] During the wastewater treatment process, aeration is performed at the cathode to provide an oxygen-containing environment, and an electrochemical workstation is used as a power source.
[0070] In certain embodiments of the present invention, the pH of the electrolyte is 7; the content of metronidazole in the electrolyte is 20 mg L -1 , the content of sodium sulfate is 0.1 mol L -1 .
[0071] In certain embodiments of the present invention, the aeration flow rate at the cathode is maintained at 300 mL min -1 .
[0072] In certain embodiments of the present invention, during the wastewater treatment process, the current density is 10 mA cm -2 .
[0073] Compared with the prior art, the present invention provides a three-dimensional porous metal-free electrode, which is prepared by freeze-drying and pyrolysis of melamine foam after being impregnated with a precursor solution; the precursor solution includes nitrogen-containing compounds and boron-containing compounds. The electrode material prepared by the present invention can improve the degradation efficiency of organic pollutants by strengthening the mass transfer process and charge distribution control strategy, and the metal-free electro-Fenton process reflects the environmentally friendly characteristics of its reaction system.
[0074] The present invention has no particular limitation on the sources of the raw materials used above, and they can be generally commercially available.
[0075] In order to further illustrate the present invention, a three-dimensional porous metal-free electrode, a preparation method and applications thereof provided by the present invention are described in detail below in combination with embodiments, but it should not be construed as limiting the scope of protection of the present invention.
[0076] Comparative Example 1
[0077] Pyrolysis preparation of melamine foam:
[0078] Commercially available melamine foam (density 8kg / m 3 ) was cut into a specific size of 5 cm × 2 cm × 1 cm, placed in a nitrogen atmosphere, heated to 900 ° C at 5 ° C / min, and kept at 900 ° C for 2 h for pyrolysis treatment to obtain a CF electrode. Among them, the scanning electron microscopy (SEM) of the initial melamine foam is as follows Figure 1 As shown, Figure 1 is the SEM image of the initial melamine foam of Comparative Example 1 of the present invention; Figure 2 As shown; Figure 2 This is the SEM image of the CF electrode of Comparative Example 1 of the present invention.
[0079] from Figure 1 and Figure 2 It can be seen that both melamine foam and the prepared CF present a porous network structure.
[0080] Comparative Example 2
[0081] Preparation of N-doped electrodes:
[0082] Ultrapure water was used to prepare 18 mL of homogeneous aqueous solution containing 12 mmol (1.3 g) of PVP; melamine foam (density 8 kg / m 3) was cut into a specific size of 5cm×2cm×1cm and then immersed in the homogeneous aqueous solution for 15 minutes; after the immersion, the immersed melamine foam was pre-frozen at -80°C for 8 hours, and then kept at -60°C in a freeze dryer for 60 hours; finally, the freeze-dried melamine foam was heated to 900°C at 5°C / min in a nitrogen atmosphere and kept at 900°C for 2 hours for pyrolysis treatment to obtain an electrode N / CF. The SEM image of the N / CF electrode is shown in FIG. Figure 3 shown. Figure 3 This is the SEM image of the N / CF electrode of Comparative Example 2 of the present invention.
[0083] from Figure 3 It can be seen that the prepared N / CF presents an interwoven porous structure, and a large number of film-like structures appear in the skeleton, which can cause partial pore blockage to a certain extent.
[0084] Example 1
[0085] Preparation of N, B co-doped electrode (NB / CF):
[0086] Ultrapure water was used to prepare 18 mL of a homogeneous aqueous solution containing 12 mmol (1.3 g) of PVP and 0.3 mmol (18 mg) of H3BO3; melamine foam (density 8 kg / m 3 ) is cut into a specific size of 5cm×2cm×1cm and then immersed in the homogeneous aqueous solution for 15min; after the immersion, the immersed melamine foam is pre-frozen at -80°C for 8h, and then kept at -60°C in a freeze dryer for 60h; finally, the freeze-dried melamine foam is heated to 900°C at 5°C / min in a nitrogen atmosphere, and kept at 900°C for 2h for pyrolysis treatment to obtain a three-dimensional porous metal-free electrode NB / CF.
[0087] The SEM image of the NB / CF electrode is as follows Figure 4 shown. Figure 4 This is a SEM image of the NB / CF electrode of Example 1 of the present invention.
[0088] from Figure 4 It can be seen that the prepared NB / CF electrode maintains an interwoven porous structure, the film structure in its skeleton is relatively reduced and the nodules are fuller, indicating that the introduction of heteroatom B is conducive to maintaining developed three-dimensional pores, and the presence of full nodules tends to form a more stable electrode structure.
[0089] The XPS pattern of the NB / CF electrode is as follows: Figure 5 shown. Figure 5 This is the XPS graph of the NB / CF electrode of Example 1 of the present invention. Figure 5The C1s spectrum of NB / CF in (a) contains characteristic peaks such as C=C (284.65 eV), CB (284.3 eV), CN (285.7 eV) and C-OH (287 eV). Figure 5 The N1s spectrum of NB / CF in (b) can be fitted into five characteristic peaks at 397.6 eV, 398.7 eV, 399.6 eV, 400.6 eV and 402.4 eV, which belong to NB, pyridinic N, pyrrolic N, graphitic N and N-oxide, respectively. Figure 5 The peaks at 189.5 eV, 191.0 eV and 192.0 eV in the B1s spectrum of NB / CF in (c) can be attributed to BC3, BN and BO. Figure 5 (d) The O1s spectrum of NB / CF shows the crystal oxygen, O - / O2 2- The peaks of OH and H2O are located at 529.6eV, 530.7eV, 531.7eV and 533.3eV respectively. Figure 5 It can be seen that nitrogen and boron elements have been successfully doped into the NB / CF electrodes, among which the catalytic active sites dominated by BC3, graphitic N and pyridinic N may play an important role in improving the electro-Fenton performance.
[0090] Comparative Example 3
[0091] Preparation of N, B co-doped electrode (NB / CF1):
[0092] Ultrapure water was used to prepare 18 mL of a homogeneous aqueous solution containing 12 mmol (1.3 g) of PVP and 1.2 mmol (72 mg) of H3BO3; melamine foam (density 8 kg / m 3 ) is cut into a specific size of 5cm×2cm×1cm and then immersed in the homogeneous aqueous solution for 15 minutes; after the immersion, the immersed melamine foam is pre-frozen at -80°C for 8 hours, and then kept at -60°C in a freeze dryer for 60 hours; finally, the freeze-dried melamine foam is heated to 900°C at 5°C / min in a nitrogen atmosphere, and is kept at 900°C for 2 hours for pyrolysis treatment to obtain a three-dimensional porous metal-free electrode NB / CF1.
[0093] The SEM of the NB / CF1 electrode is as follows Figure 6 shown. Figure 6 This is a SEM image of the NB / CF1 electrode of Comparative Example 3 of the present invention.
[0094] from Figure 6 It can be seen that the prepared NB / CF1 maintains an interwoven porous structure, and there are few film structures and large joints in its skeleton due to the introduction of a large amount of B.
[0095] Example 2
[0096] Preparation of N, B co-doped electrode (NB / CF2):
[0097] Ultrapure water was used to prepare 18 mL of a homogeneous aqueous solution containing 12 mmol (1.3 g) of PVP and 0.6 mmol (36 mg) of H3BO3; melamine foam (density 8 kg / m 3 ) is cut into a specific size of 5cm×2cm×1cm and then immersed in the homogeneous aqueous solution for 15 minutes; after the immersion is completed, the immersed melamine foam is pre-frozen at -80°C for 8 hours, and then kept at -60°C in a freeze dryer for 60 hours; finally, the freeze-dried melamine foam is heated to 900°C at 5°C / min in a nitrogen atmosphere, and is kept at 900°C for 2 hours for pyrolysis treatment to obtain a three-dimensional porous metal-free electrode NB / CF2.
[0098] The SEM of the NB / CF2 electrode is as follows Figure 7 shown. Figure 7 This is a SEM image of the NB / CF2 electrode of Example 2 of the present invention.
[0099] from Figure 7 It can be seen that the prepared NB / CF2 maintains an interwoven porous structure, and as the introduced B content decreases, the film structure in its skeleton gradually increases and the nodules gradually shrink.
[0100] Example 3
[0101] Preparation of N, B co-doped electrode (NB / CF3):
[0102] Ultrapure water was used to prepare 18 mL of a homogeneous aqueous solution containing 12 mmol (1.3 g) of PVP and 0.2 mmol (12 mg) of H3BO3; melamine foam (density 8 kg / m 3 ) is cut into a specific size of 5cm×2cm×1cm and then immersed in the homogeneous aqueous solution for 15 minutes; after the immersion, the immersed melamine foam is pre-frozen at -80°C for 8 hours, and then kept at -60°C in a freeze dryer for 60 hours; finally, the freeze-dried melamine foam is heated to 900°C at 5°C / min in a nitrogen atmosphere, and is kept at 900°C for 2 hours for pyrolysis treatment to obtain a three-dimensional porous metal-free electrode NB / CF3.
[0103] The SEM of the NB / CF3 electrode is as follows Figure 8 shown. Figure 8 This is a SEM image of the NB / CF3 electrode of Example 3 of the present invention.
[0104] from Figure 8It can be seen that the prepared NB / CF3 maintains an interwoven porous structure, and as the introduced B content further decreases, the film structure in its skeleton further increases and the nodules further shrink.
[0105] Comparative Example 4
[0106] Preparation of N, B co-doped electrode (NB / CF4):
[0107] Ultrapure water was used to prepare 18 mL of a homogeneous aqueous solution containing 12 mmol (1.3 g) of PVP and 0.15 mmol (9 mg) of H3BO3; melamine foam (density 8 kg / m 3 ) is cut into a specific size of 5cm×2cm×1cm and then immersed in the homogeneous aqueous solution for 15 minutes; after the immersion, the immersed melamine foam is pre-frozen at -80°C for 8 hours, and then kept at -60°C in a freeze dryer for 60 hours; finally, the freeze-dried melamine foam is heated to 900°C at 5°C / min in a nitrogen atmosphere, and is kept at 900°C for 2 hours for pyrolysis treatment to obtain a three-dimensional porous metal-free electrode NB / CF4.
[0108] The SEM of the NB / CF4 electrode is as follows Fig. 9 shown. Fig. 9 This is a SEM image of the NB / CF4 electrode of Comparative Example 4 of the present invention.
[0109] from Fig. 9 It can be seen that due to the extremely small amount of B doping, the prepared NB / CF4 has a large number of thin film structures, and the microstructure is similar to that of N / CF.
[0110] The XRD patterns of the electrodes prepared in Examples 1 to 3 and Comparative Examples 1 to 4 are as follows: Fig.10 shown. Fig.10 The XRD diagrams of the electrodes prepared in Examples 1 to 3 and Comparative Examples 1 to 4 of the present invention are shown.
[0111] from Fig.10 It can be seen that compared with CF (23°), the diffraction peak intensity of the electrodes prepared in Examples 1 to 3 and Comparative Examples 2 to 4 increases and slightly shifts, indicating that their degree of graphitization increases. This is because the doped N has a higher electronegativity, which increases the stacking order and conductivity of the quasi-graphitized carbon layer. In addition, the diffraction peaks of the electrodes prepared in Examples 1 to 3 and Comparative Examples 3 to 4 at 26.6°, 41.7° and 43.8° correspond to the (002) crystal plane, (100) crystal plane and (101) crystal plane of boron nitride (BN, PDF 85-1068), respectively, indicating the successful doping of B.
[0112] Application Examples
[0113] Electro-Fenton catalytic performance test
[0114] Take the electrodes provided in Examples 1 to 3 and Comparative Examples 1 to 4 respectively, use the electrodes as cathodes and Pt as anodes and place them in single-chamber electrolytic cells. The pH of the reaction solution is 7, and the content of mg L -1 Metronidazole and 0.1 mol L -1 Na2SO4, maintain the aeration flow rate at the cathode at 300mLmin -1 . Current density 10 mA cm -2 The electro-Fenton degradation reaction was started under the conditions, and the concentration decay trend of the pollutant metronidazole was analyzed by liquid chromatography. The results are shown in Fig.11 . Fig.11 The electro-Fenton performance diagram of the electrodes prepared in Examples 1 to 3 of the present invention and Comparative Examples 1 to 4 is shown.
[0115] Depend on Fig.11 It can be seen that with the gradual increase of the introduction ratio of B, the electro-Fenton degradation efficiency shows a trend of first increasing and then decreasing, among which NB / CF shows the best electro-Fenton activity, and the pollutants can be almost completely removed in 60 minutes. This result shows that appropriate B doping is beneficial to improving the electro-Fenton efficiency, and the three-dimensional pore mass transfer process induced by it and the charge regulation of doped active sites (such as BCCC-graphite N and BCCC-pyridine N, etc.) synergistically improve the catalytic activity.
[0116] Electro-Fenton stability performance test
[0117] The NB / CF electrode of Example 1 was used as the cathode and Pt was used as the anode and placed in a single-chamber electrolytic cell. The pH of the reaction solution was 7 and contained 20 mg L -1 Metronidazole and 0.1 mol L -1 Na2SO4, maintain the aeration flow rate at the cathode at 300 mL min -1 . Current density 10 mA cm -2 The electro-Fenton degradation reaction was started under the same experimental conditions. After the reaction, the electrode was simply cleaned. The electro-Fenton degradation experiment was repeated under the same experimental conditions. The concentration decay trend of the pollutant metronidazole during each reaction was analyzed by liquid chromatography. The results are shown in Fig.12 . Fig.12 This is the electro-Fenton stability performance diagram of the NB / CF electrode of Example 1 of the present invention.
[0118] Depend on Fig.12 It can be seen that after 10 cycles of the electro-Fenton degradation reaction, the removal rate of pollutants did not show a significant downward trend, and the metronidazole removal rate was still as high as 97.8%, indicating that the NB / CF electrode has significant stability.
[0119] The description of the above embodiments is only used to help understand the method of the present invention and its core idea. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features disclosed herein.
Claims
1. Application of a three-dimensional porous metal-free electrode as an electro-Fenton cathode in electro-Fenton degradation and removal of metronidazole in wastewater treatment, characterized in that: The method for preparing the three-dimensional porous metal-free electrode comprises the following steps: A) immersing the melamine foam in a precursor solution for a period of time; the precursor solution comprises a nitrogen-containing compound and a boron-containing compound; the molar ratio of the nitrogen-containing compound to the boron-containing compound is 10-80:1; B) pre-freezing the impregnated melamine foam and then freeze-drying it; C) subjecting the freeze-dried melamine foam to pyrolysis in an inert gas atmosphere to obtain a three-dimensional porous metal-free electrode.
2. The use according to claim 1, characterized in that: The nitrogen-containing compound comprises at least one of polyvinyl pyrrolidone, urea, aniline, tert-butylamine, melamine, dicyandiamide, ammonium chloride, ammonium carbonate and chitosan; The boron-containing compound comprises at least one of boric acid, borax, boron trioxide, borane, sodium borohydride, triphenyl boroxine, triethyl borate and 3-aminophenylboronic acid.
3. The use according to claim 1, characterized in that: The solvent in the precursor solution is ultrapure water.
4. The use according to claim 1, characterized in that: In step A), the immersion temperature is room temperature and the immersion time is 10 to 20 minutes.
5. The use according to claim 1, characterized in that: In step B), the pre-freezing temperature is -78 to -82°C and the time is 6 to 10 hours; The freeze-drying temperature is -70 to -50°C and the time is 55 to 65 hours.
6. The use according to claim 1, characterized in that: In step C), the inert gas is nitrogen.
7. The use according to claim 1, characterized in that: In step C), the pyrolysis treatment temperature is 850-950°C and the time is 1.5-2.5 h; The temperature of the freeze-dried melamine foam is raised to the pyrolysis treatment temperature in an inert gas atmosphere at a heating rate of 4-6°C / min.