A biodegradable meltblown nonwoven fabric material and its preparation method and application

By using a blended material of biodegradable resin and polylactic acid in meltblown nonwovens, combined with compatibility agents and lubricants, the environmental pollution, mechanical properties and production costs of polypropylene meltblown nonwovens are solved, and the problem of environmental pollution, mechanical properties and production costs of polypropylene meltblown nonwovens is achieved. It has the effect of high-efficiency filtration and low ventilation resistance, and is suitable for a variety of application areas.

CN115819931BActive Publication Date: 2024-11-08CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202111093398.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-09-17
Publication Date
2024-11-08
Estimated Expiration
2041-09-17

AI Technical Summary

Technical Problem

The existing polypropylene meltblown nonwoven fabric materials have problems such as environmental pollution, insufficient mechanical properties, high production costs, and further improvement in filtration and mechanical properties.

Method used

Using a blended material of biodegradable resins PBAT, PBS and polylactic acid, it is processed through twin screw granulation and meltblown processes, combining compatibility agents, lubricants and antioxidants to form excellent filtration performance, air permeability and Meltblown nonwoven fabrics with mechanical properties do not require electrostatic electret treatment, reducing energy consumption.

Benefits of technology

Biodegradable meltblown nonwovens with high efficiency filtration performance, low ventilation resistance and good mechanical properties are obtained, which is suitable for wide application in air filtration, adsorption materials, mask materials and other fields, reducing production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115819931B_ABST
    Figure CN115819931B_ABST
Patent Text Reader

Abstract

The present invention discloses a biodegradable melt-blown nonwoven fabric material and its preparation method and application, which is composed of the following components: biodegradable resin, polylactic acid, compatibilizer, lubricant, chain extender and antioxidant. The preparation process of the above material is as follows: the raw materials of each component are mixed evenly in proportion, and the biodegradable slices are obtained by twin-screw blending and granulation, and the biodegradable melt-blown nonwoven fabric is obtained by melt-blown nonwoven process. The degradable melt-blown nonwoven material provided by the present invention has a biodegradable function, as well as excellent filtering performance, air permeability and mechanical properties, and is hydrophilic, and is more suitable for application in the fields of air filtration, adsorption materials, mask materials, wipes, various packaging materials and medical sanitary materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polymer material application, and relates to a biodegradable melt-blown nonwoven fabric material and a preparation method and application thereof, and more specifically, relates to a processing method for promoting the application of blended biodegradable materials in the field of melt-blown nonwoven materials. Background Art

[0002] Meltblown nonwoven fabrics are made by meltblowing polymers directly into mesh-shaped nonwoven fabrics, and their raw materials are generally polypropylene. Since the meltblown processing technology uses hot air to blow and does not have a long drafting tunnel, the process flow of meltblown nonwoven technology is very short. It is known as the one-step polymer direct web-forming method with the shortest process, which makes it have the advantages of high output, low cost, high efficiency, solvent-free, wide application, and multiple sources of raw materials. The biggest feature of meltblown nonwoven fabrics is that the fibers are very fine, with a diameter of only a few microns. After self-bonding, the structure is fluffy, the porosity is high, the average pore size is small, and it has very good filtration, shielding, insulation and oil absorption. Application characteristics. Therefore, meltblown nonwoven fabrics are widely used in medical and industrial masks, thermal insulation materials, filter materials, medical and sanitary materials, oil-absorbing materials, wipes, battery separators, and sound insulation materials.

[0003] At present, there are mainly the following problems in improving polypropylene meltblown nonwoven materials:

[0004] First, with the rapid development of industry and the growing market of meltblown nonwovens, meltblown nonwoven materials bring great convenience to people's lives, but also threaten the living environment of mankind. The waste of polypropylene meltblown nonwoven materials will produce harmful gases after incineration. If it is difficult to degrade if buried, it will cause serious environmental pollution problems. This is a very worrying problem that needs to be solved urgently. In order to solve this problem, Chinese patent CN103073868B discloses a biodegradable meltblown nonwoven slice and a preparation method thereof, wherein polypropylene carbonate and polypropylene meltblown nonwoven slices are melt-blended to prepare a biodegradable meltblown nonwoven slice with excellent performance. Although its mechanical properties and thermal properties are excellent, it does not mention the specific performance of the meltblown nonwoven fabric, and due to the presence of polypropylene, its degradable performance needs to be improved.

[0005] Second, polypropylene melt-blown nonwoven fabrics still have problems such as insufficient strength and low elongation at break, which are mainly manifested in that the fabric feels hard, which limits subsequent processing and use. Chinese patents CN105086394B and CN107227555A both improve the mechanical properties of melt-blown nonwoven materials by adding modified nano-inorganic materials to the materials. However, the surface modification process of nano-inorganic materials is complicated and consumes a large amount of solvent. Nano-inorganic materials are prone to agglomeration during the blending process, and inorganic particles are prone to filter screen and nozzle clogging during the melt-blowing process. For example, Chinese patent CN105086394B discloses a biodegradable composite material containing SiO2 for melt-blown nonwoven fabrics and a preparation method. SiO2 particles are added to the biodegradable resin through nano-composite modification technology to improve the filtration efficiency of the biodegradable melt-blown nonwoven fabric and improve the mechanical properties of the biodegradable melt-blown nonwoven fabric. However, it does not solve the incompatibility problem between several biodegradable resins. It uses a high PLA content, and the nano-SiO2 particles are easy to agglomerate during the blending and granulation process. It requires the use of a large amount of alcohol and water solvents, and the surface of the nano-SiO2 particles needs to be chemically modified. The process is cumbersome and complicated, with low output, and will also cause a lot of resource waste and energy consumption, which is not environmentally friendly.

[0006] Third, there are few studies on the application of biodegradable materials in meltblowing. Chinese patent CN102295825A discloses a biodegradable composition and its preparation method. The disclosed biodegradable composition is composed of biodegradable homopolyester (A), biodegradable copolyester (B) and chain extender (C). The total weight of the three is 100 parts by mass, containing 95.0 to 99.9 parts (A + B) and 0.1 to 5.0 parts C, wherein the ratio of A: B is 1: 9 to 9: 1. This patent is mainly designed to solve the problems of unstable degradation rate of biodegradable materials, narrow application of processing physical properties, and poor resistance to moisture and heat, hydrolysis, and oxidation. The invention finally obtains a material with moderate biodegradation rate and good physical processing performance, wherein the main evaluation indicators are mechanical tensile properties, mechanical retention rate and biodegradation rate. This material is mainly used in the fields of blow molding, extrusion molding, injection molding and spinning molding, but it does not mention the application and application prospects in the field of meltblown nonwovens. This invention obviously does not solve the problem of incompatibility between different biodegradable materials, and is irrelevant to the technical problem that the present invention is intended to solve and the technical effect obtained.

[0007] Fourth, when melt-blown nonwovens are used as filter materials, their filtering performance and mechanical properties have attracted much attention. As far as the prior art is concerned, melt-blown nonwovens need to obtain higher filtering efficiency and better air permeability, and inevitably add various types of inorganic or organic electrets, and add tens of thousands of volts of electrostatic electret effect, which is not only costly but also consumes a lot of energy in the actual production process. For example, Chinese patent CN104711764B discloses a high-strength long-acting electret ultrafine fiber PLA melt-blown nonwoven material and a preparation method thereof, wherein PLA slices and nanoparticle additives are blended, and a degradable melt-blown nonwoven material with good mechanical properties and long-acting electret function is obtained by an improved melt-blown processing technology. However, the mechanical properties of the high-weight PLA melt-blown nonwoven fabric obtained are not very excellent, and the comprehensive performance needs to be further improved, and the production cost of this method is very high. Summary of the invention

[0008] One of the purposes of the present invention is to provide a biodegradable meltblown nonwoven fabric material, which is suitable for meltblowing process processing. The prepared nonwoven fabric has biodegradability, excellent filtering performance, air permeability and mechanical properties, and is hydrophilic.

[0009] The second object of the present invention is to provide a method for preparing the above-mentioned biodegradable melt-blown nonwoven fabric material.

[0010] The third object of the present invention is to provide the application of the above-mentioned biodegradable melt-blown nonwoven fabric material.

[0011] In summary, the technical problem to be solved by this technical solution is to provide a biodegradable meltblown nonwoven fabric material, which has excellent filtration performance, air permeability and mechanical properties, while reducing production costs and can be widely used in the field of nonwoven fabrics.

[0012] The purpose of the present invention can be achieved through the following technical solutions:

[0013] A biodegradable meltblown nonwoven fabric material comprising the following components:

[0014]

[0015] Preferably, the material comprises the following components:

[0016]

[0017] In the technical solution of the present invention: the biodegradable resin is at least one of PBAT, PBST, PBSA and PBS.

[0018] Preferably, the melt index of the biodegradable resin is 100-500 g / 10 min at 210° C. and 2.16 kg.

[0019] Furthermore: the melt index of the biodegradable resin is 300-500 g / 10 min at 210° C. and 2.16 kg.

[0020] Most preferably, the biodegradable resin is PBAT produced by Yizheng Chemical Fiber and / or PBS produced by Yizheng Chemical Fiber.

[0021] In the technical solution of the present invention: the melt index of the polylactic acid is 80-400g / 10min at 250°C and 2.16kg.

[0022] Furthermore: the melt index of the polylactic acid is 50-400 g / 10 min at 250° C. and 2.16 kg; the molecular weight of the polylactic acid is between 100,000 and 130,000, and the melting point is 160° C.-170° C.

[0023] Most preferably, the polylactic acid is PLA-L105 produced by Suzhou Lvbo Degradable Materials Co., Ltd.

[0024] In the technical solution of the present invention: the compatibilizer is at least one of maleic anhydride, benzoyl peroxide, tetrabutyl titanate and polyacid; the lubricant is selected from at least one of zinc stearate, calcium stearate and magnesium stearate; the chain extender is selected from at least one of ADR4370S and KL-E4370; the antioxidant is at least one of antioxidant 168 and antioxidant 1010.

[0025] In some preferred technical solutions: the lubricant is selected from at least one of zinc stearate, calcium stearate, and magnesium stearate and mixed with one of the chain extenders ADR4370S and KL-E4370 in a ratio of 1:0.5-1.5; the antioxidant is antioxidant 168 and antioxidant 1010 mixed in a ratio of 1:0.5-1.5.

[0026] In some of the most preferred technical solutions: the lubricant is selected from at least one of zinc stearate, calcium stearate, and magnesium stearate and mixed with one of the chain extenders ADR4370S and KL-E4370 in a 1:1 ratio; the antioxidant is antioxidant 168 and antioxidant 1010 mixed in a 1:1 ratio.

[0027] The second object of the present invention is to provide a method for preparing the above-mentioned biodegradable melt-blown nonwoven fabric material, comprising pre-treating and stirring components including a biodegradable resin, polylactic acid (PLA), a compatibilizer, a lubricant and an antioxidant to obtain a mixed material, and subjecting the mixture to twin-screw granulation and melt-blowing process processing.

[0028] A method for preparing the above-mentioned biodegradable melt-blown nonwoven fabric material comprises the following steps:

[0029] S1. Prepare mixed materials:

[0030] S11, stirring and mixing the dried biodegradable resin, polylactic acid, compatibilizer, lubricant, chain extender, and antioxidant in a high-speed mixer according to a formula ratio to obtain a mixed material;

[0031] S2, twin-screw granulation of the mixed material:

[0032] The mixed material is melted, extruded, air-cooled, drawn, and cold-cut to produce biodegradable resin / PLA blended biodegradable slices;

[0033] S3, preparing melt-blown nonwoven fabric from the biodegradable resin / PLA blended biodegradable slices prepared above:

[0034] S31, drying the biodegradable resin / PLA blended biodegradable slices prepared above at 70-90° C. for 6-24 hours;

[0035] S32, melt-blown process: add the dried biodegradable resin / PLA blended biodegradable slices into the automatic hopper of the melt-blown device, send them into the screw extruder for heating and melting, flow into the pre-filter, filter out impurities in the melt, and then flow to the metering pump. The melt is pressed out to the small orifice of the spinneret die by the pressure of the metering pump. The diameter of the spinneret hole is 0.2-0.5mm. The high-speed hot compressed air on both sides of the small hole will perform hot air high-speed drawing on the melt extruded from the spinneret. The obtained melt-blown ultrafine fibers are cooled and crystallized in a short time under the action of side-blown cold wind. The fibers gather on the mesh curtain with a distance DCD of 160-250mm from the die head, wherein: the suction wind speed under the mesh is 1000-3000rpm; at the same time, the running speed of the round net is 3-10m / min, and the winding speed is 3-10m / min to form an ultrafine fiber melt-blown nonwoven fabric with good mechanical properties;

[0036] S33. The nonwoven fabric obtained above does not need to be subjected to electret treatment by an electrode device, which greatly saves energy consumption. Finally, the meltblown nonwoven material product is obtained by winding it into a roll on a roll-forming machine and slitting it online.

[0037] In some specific technical solutions, the method includes the following steps:

[0038] S1. Prepare mixed materials:

[0039] S11, stirring and mixing the dried biodegradable resin, polylactic acid, compatibilizer, lubricant, chain extender, and antioxidant in a high-speed mixer according to a formula ratio to obtain a mixed material;

[0040] S2, twin-screw granulation of the mixed material:

[0041] Twin-screw granulation process: the mixed material obtained above is added through the silo and stirred continuously, the granulation screw temperature is 180-230°C, the screw speed is 200-300r / min, and the metering pump speed is 100-300Kg / h; the mixed material is extruded, air-cooled, stretched, and cold-cut to make biodegradable resin / PLA blended biodegradable slices;

[0042] S3, preparing melt-blown nonwoven fabric from the biodegradable resin / PLA blended biodegradable slices prepared above:

[0043] S31, drying the biodegradable resin / PLA blended biodegradable slices prepared above at 70-90° C. for 6-24 hours;

[0044] S32, melt-blown process: add the dried biodegradable resin / PLA blended biodegradable slices into the automatic hopper of the melt-blown device, send them into the screw extruder for heating and melting, flow into the pre-filter, filter out impurities in the melt, and then flow to the metering pump. The melt is pressed out to the small orifice of the spinneret die by the pressure of the metering pump. The diameter of the spinneret hole is 0.2-0.5mm. The high-speed hot compressed air on both sides of the small hole will perform hot air high-speed drawing on the melt extruded from the spinneret. The obtained melt-blown ultrafine fibers are cooled and crystallized in a short time under the action of side-blown cold wind. The fibers gather on the mesh curtain with a distance DCD of 160-250mm from the die head, wherein: the suction wind speed under the mesh is 1000-3000rpm; at the same time, the running speed of the round net is 3-10m / min, and the winding speed is 3-10m / min to form an ultrafine fiber melt-blown nonwoven fabric with good mechanical properties;

[0045] S33. The nonwoven fabric obtained above does not need to be subjected to electret treatment by an electrode device, which greatly saves energy consumption. Finally, the meltblown nonwoven material product is obtained by winding it into a roll on a roll-forming machine and slitting it online.

[0046] In some specific technical solutions: in the S32, the parameters are set as follows:

[0047]

[0048] In the preparation method of the present invention, the following melt-blowing process parameters are specifically adjusted, and a finer and more uniform fiber structure is obtained by matching and adjusting the melt-blowing process parameters, thereby improving the filtration performance of the melt-blown nonwoven material. According to the properties of different materials, the present invention adjusts the process parameters such as screw temperature, die head temperature, DCD, air heater outlet wind temperature and wind speed, side blowing fan speed, under-net suction wind speed, and round net speed.

[0049] Functional description of each component in the formula of the present invention:

[0050] First, the chemical structure of biodegradable resin is stable. Due to its structure, the trap is generally deeper, and the ability to capture and store charges is stronger, making it a better electret. Since biodegradable resin crystallizes slowly, charge trap sources can be continuously formed during the crystallization process. As the grain structure becomes more perfect, the charge capture stability becomes better. Biodegradable resin with a melt index of 300-500g / 10min has good fluidity, which is more conducive to obtaining finer fibers under the melt-blown process. The porous structure of the formed melt-blown ultrafine fibers can form a charge capture space and obtain a melt-blown nonwoven material with high filtration efficiency. In addition, biodegradable resin has good mechanical properties, and can obtain a melt-blown nonwoven material with good mechanical properties, soft hand feel, and good hydrophilicity.

[0051] Second, PLA is a non-crystalline material. PLA with a melt index of 50-400g / 10min is selected and compounded with biodegradable resin to obtain biodegradable materials with different ratios. Crystalline and amorphous mixed fibers are obtained through melt-blowing process. The charge will accumulate on the interface between the crystalline and amorphous regions, and the charge will be retained inside the three-dimensionally aggregated high-porosity fibers, which is conducive to obtaining biodegradable melt-blown cloth materials with excellent filtration performance. In addition, the mechanical properties of PLA itself are poor. Through the ratio of biodegradable resin, PLA and additives, a melt-blown nonwoven material with excellent filtration performance and mechanical properties and soft feel is obtained.

[0052] Third, the compatibilizer can solve the incompatibility problem between biodegradable resin and PLA, avoid the phenomenon of fiber discontinuity and unevenness in the melt-blown process, thereby improving the filtration efficiency and mechanical properties of melt-blown nonwoven materials.

[0053] Fourth, stearate can be used as an additive to promote the crystallization of materials, increase the crystallinity and α-crystal ratio of materials, increase the grain size, effectively improve the flow properties of materials, and the effect becomes more obvious with the increase of concentration, thereby improving the filtration efficiency and electrical storage performance of materials. The addition of appropriate chain extenders ADR4370S or KL-E4370 not only plays the role of lubricant and nucleating agent, but also interacts with biodegradable resin and PLA, significantly improving the compatibility and mechanical properties of biodegradable resin and PLA blending system.

[0054] Fifth, antioxidants are mainly used to prevent PLA from decomposing due to heat, so as not to reduce the physical properties of the material.

[0055] Key points of the invention that are different from the closest prior art:

[0056] First, the formula of the degradable melt-blown nonwoven material provided by the present invention is different from the prior art. The biodegradable material and PLA are blended to give the melt-blown nonwoven material a biodegradable function, and the proportion of polylactic acid in the mixture is 10-40%. By compounding a compatibilizer, a lubricant, and an antioxidant, a material with uniform melt and good fluidity is obtained. Without adding an electret, the filtration efficiency and charge storage capacity of the melt-blown nonwoven material are improved, the feel and mechanical properties of the material are improved, the medical protection performance of the material is enhanced, and the application field of the material is broadened. The present invention has simple equipment, short process flow, low energy consumption, and does not use any solvent.

[0057] Second, the preparation method of the degradable melt-blown nonwoven material provided by the present invention is different from the prior art. The prior art does not have a processing method that can enable the melt-blown nonwoven material to obtain excellent filtration efficiency and lower ventilation resistance without additionally adding electret and using electrostatic electret.

[0058] Third, the degradable meltblown nonwoven material provided by the present invention has biodegradable function, as well as excellent filtering performance, air permeability and mechanical properties, and is hydrophilic, and is more suitable for application in air filtration, adsorption materials, mask materials, wiping cloths, various packaging materials, and medical and sanitary materials.

[0059] Beneficial effects of the present invention:

[0060] The present invention produces a degradable melt-blown nonwoven material. The present invention obtains a degradable melt-blown nonwoven material with excellent filtering performance, small ventilation resistance, excellent mechanical properties and hydrophilicity without adding an electret and using an electrostatic electret. BRIEF DESCRIPTION OF THE DRAWINGS

[0061] Figure 1 This is a scanning electron micrograph of the product of Example 2 of the present invention, with average fiber diameter (μm) / standard deviation 2.01 / 0.98.

[0062] Figure 2 This is a scanning electron micrograph of the product of Comparative Example 1 of the present invention, with an average fiber diameter (μm) / standard deviation of 2.43 / 1.42.

[0063] Figure 3 This is a scanning electron micrograph of the product of Comparative Example 2 of the present invention, with an average fiber diameter (μm) / standard deviation of 8.6 / 12.7.

[0064] Figure 4 This is a scanning electron micrograph of the product of Comparative Example 3 of the present invention, with an average fiber diameter (μm) / standard deviation of 3.01 / 23.2.

[0065] Figure 5It is a cross-sectional view of the slices of comparative examples 1 to 2 and the example products of the present invention. DETAILED DESCRIPTION

[0066] The present invention is further described below in conjunction with embodiments, but the protection scope of the present invention is not limited thereto:

[0067] The degradable meltblown nonwoven fabric material of the present invention is tested according to the following standards:

[0068] Tensile strength: GB / T1040-2006.

[0069] Weight: FZ / T 64078-2019.

[0070] Filtration resistance: FZ / T 64078-2019, test substance NaCl, particle size 0.3μm, test flow rate 32L / min.

[0071] Filtration efficiency: FZ / T 64078-2019, test substance NaCl, particle size 0.3μm, test flow rate 32L / min.

[0072] Average fiber diameter: 30 fibers were selected and observed using a scanning electron microscope to measure their average diameter.

[0073] Raw materials used in the embodiments and comparative examples:

[0074] Polypropylene (PP): Z-1500 from Shandong Dawn Polymer Materials Co., Ltd.

[0075] Polylactic acid (PLA): PLA-L105 from Suzhou Lvbo Degradable Materials Co., Ltd.

[0076] Biodegradable resin: PBAT, PBS, produced by Yizheng Chemical Fiber.

[0077] Electret: tourmaline powder, commercially available.

[0078] Compatibilizer: Maleic anhydride, produced by Yizheng Chemical Fiber.

[0079] Lubricant: magnesium stearate, commercially available; ADR4370S, produced by BASF.

[0080] Antioxidants: Antioxidant 168 and Antioxidant 1010, commercially available

[0081] Embodiment 1:

[0082] Prepare the materials and components according to the ratio in Table 1 and proceed as follows:

[0083] S1. Prepare mixed materials:

[0084] S11, drying the biodegradable resin PBAT at 80° C. for 14 h, and drying the PLA at 110° C. for 14 h to obtain a dry biodegradable material;

[0085] S12, stirring and uniformly mixing the biodegradable resin, polylactic acid, compatibilizer, lubricant, chain extender, and antioxidant in a high-speed mixer according to a formula ratio to obtain a mixed material;

[0086] S2, twin-screw granulation of the mixed material:

[0087] Twin-screw granulation process: The above-obtained mixed material is added through the silo and stirred continuously. The granulation screw temperature is 195°C in zone 1, 210°C in zone 2, 230°C in zones 3-9, and 210°C in zone 10. The screw speed is 250r / min and the metering pump speed is 150Kg / h. The mixed material is extruded, air-cooled, stretched and cold-cut to produce biodegradable PBAT / PLA blended biodegradable slices.

[0088] S3, preparing melt-blown nonwoven fabric from the biodegradable PBAT / PLA blend slices prepared above:

[0089] S31, drying the biodegradable PBAT / PLA blended slices prepared above at 85° C. for 12 h.

[0090] S32, melt-blowing process: add the dried biodegradable PBAT / PLA blended slices into the automatic silo of the melt-blowing device, send them into the screw extruder for heating and melting, the screw temperature is 180℃ in zone 1, 200℃ in zone 2, 230℃ in zone 3, 245℃ in zones 4-7, then the melt flows into the pre-filter to filter out impurities in the melt, and then flows to the metering pump with a flow rate of 6rpm. The melt is pressed out to the small orifice of the spinneret die (die temperature 245℃) by the pressure of the metering pump, and the spinneret is formed. The hole diameter is 0.28mm. The high-speed hot compressed air (240℃) on both sides of the small hole will perform hot air high-speed drawing on the melt extruded from the spinneret to obtain melt-blown ultrafine fibers. The fibers are cooled and crystallized in a short time. The side blowing fan speed is 2100rpm, and the suction fan speed under the net is 2700rpm. The fibers gather on the mesh curtain, the receiving distance DCD is 190mm, and the round net speed is 4m / mim, forming an ultrafine fiber melt-blown nonwoven fabric with good mechanical properties.

[0091] S33, the nonwoven fabric obtained above is rolled up on a roll-forming machine and cut online to obtain a finished meltblown nonwoven material.

[0092] The test results of the obtained biodegradable melt-blown nonwoven fabric weight, filtration resistance, filtration efficiency, tensile strength, tensile elongation at break and average fiber diameter are shown in Table 3.

[0093] Embodiment 2:

[0094] The materials and components are prepared according to the ratios in Table 1. The conditions of the preparation method are the same as those in Example 1, except that in step S32: the screw temperature is 180°C in zone 1, 200°C in zone 2, 230°C in zone 3, 250°C in zones 4-7, the temperature of the stretching hot air is 245°C, the side blowing fan speed is 1900rpm, the under-net suction fan speed is 2600rpm, and the cylinder screen speed is 6m / mim.

[0095] The biodegradable melt-blown nonwoven fabric obtained (such as Figure 1 ) The test results of gram weight, filtration resistance, filtration efficiency, tensile strength, tensile elongation at break and average fiber diameter are shown in Table 3.

[0096] Embodiment 3:

[0097] The materials and components are prepared according to the ratios in Table 1. The conditions of the preparation method are the same as those in Example 1, except that in step S32: the screw temperature is 180°C in zone 1, 200°C in zone 2, 230°C in zone 3, 255°C in zones 4-7, the temperature of the stretching hot air is 250°C, the side blowing fan speed is 1800rpm, the under-net suction fan speed is 2400rpm, and the cylinder screen speed is 8m / mim.

[0098] The test results of the obtained biodegradable melt-blown nonwoven fabric weight, filtration resistance, filtration efficiency, tensile strength, tensile elongation at break and average fiber diameter are shown in Table 3.

[0099] Embodiment 4:

[0100] The materials and components are prepared according to the ratios in Table 1. The conditions of the preparation method are the same as those in Example 1, except that in step S32: the side blowing fan speed is 1800 rpm, the under-net suction fan speed is 2400 rpm, and the cylinder screen speed is 6 m / mim.

[0101] The test results of the obtained biodegradable melt-blown nonwoven fabric weight, filtration resistance, filtration efficiency, tensile strength, tensile elongation at break and average fiber diameter are shown in Table 3.

[0102] Embodiment 5:

[0103] The materials and components are prepared according to the ratios in Table 1. The conditions of the preparation method are the same as those in Example 1, except that in step S32: the screw temperature is 180°C in zone 1, 200°C in zone 2, 230°C in zone 3, 250°C in zones 4-7, the temperature of the stretching hot air is 245°C, the side blowing fan speed is 1800rpm, the under-net suction fan speed is 2500rpm, and the cylinder screen speed is 6m / mim.

[0104] The test results of the obtained biodegradable melt-blown nonwoven fabric weight, filtration resistance, filtration efficiency, tensile strength, tensile elongation at break and average fiber diameter are shown in Table 3.

[0105] Comparative Example 1:

[0106] Prepare the materials and components according to the ratio in Table 2 and proceed as follows:

[0107] S1. Prepare mixed materials:

[0108] S11, stirring and uniformly mixing polypropylene PP, electret tourmaline powder, magnesium stearate and antioxidant in a high-speed mixer according to a formula ratio to obtain a mixed material;

[0109] S2, preparing melt-blown nonwoven fabric from the mixed material:

[0110] S21, melt-blowing process: same as in Example 2;

[0111] S22. The nonwoven fabric obtained above is subjected to electret treatment by a string-drum type linear electrode device, and the electrode voltage is 30 kV, thereby obtaining a melt-blown nonwoven fabric.

[0112] S23, the nonwoven fabric obtained above is rolled up on a roll-forming machine and cut online to obtain a finished meltblown nonwoven material.

[0113] The obtained polypropylene melt-blown nonwoven fabric (such as Figure 2 ) The test results of gram weight, filtration resistance, filtration efficiency, tensile strength, tensile elongation at break and average fiber diameter are shown in Table 3.

[0114] Comparative Example 2:

[0115] Prepare the materials and components according to the ratio in Table 2 and proceed as follows:

[0116] S1, drying the biodegradable resin PBAT at 80° C. for 14 h to obtain a dry biodegradable material;

[0117] S2, melt-blown process: add the material into the automatic hopper of the melt-blown device, send it into the screw extruder for heating and melting, the screw temperature is 180℃ in zone 1, 200℃ in zone 2, 230℃ in zone 3, and 245℃ in zones 4-7, then the melt flows into the pre-filter to filter out impurities in the melt, and then flows to the metering pump, the flow rate of the metering pump is 6rpm, the melt is pressed out to the small orifice of the spinneret die by the pressure of the metering pump, the diameter of the spinneret hole is 0.28mm, and the high-speed hot compressed air on both sides of the small hole will perform hot air high-speed drawing on the melt extruded from the spinneret, the temperature of the drawing hot air is 230℃, and melt-blown ultrafine fibers are obtained. After a short period of cooling and crystallization, the side blowing fan speed is 2300rpm, the suction fan speed under the net is 2500rpm, the fibers gather on the net curtain, the receiving distance DCD is 190mm, and the round net speed is 4m / mim to form a melt-blown nonwoven fabric.

[0118] S3. The nonwoven fabric obtained above is rolled up on a roll-forming machine and cut online to obtain a finished meltblown nonwoven material.

[0119] The biodegradable melt-blown nonwoven fabric obtained (such as Figure 3 ) The test results of gram weight, filtration resistance, filtration efficiency, tensile strength, tensile elongation at break and average fiber diameter are shown in Table 3.

[0120] In addition: if the preparation process parameters are the same as those in the embodiment, this comparative example will not be able to produce a conventional meltblown nonwoven material.

[0121] Comparative Example 3:

[0122] Prepare the materials and components according to the ratio in Table 2 and proceed as follows:

[0123] S1, drying PLA at 110° C. for 14 h to obtain a dry biodegradable material;

[0124] S2, melt-blowing process: same as in Example 2;

[0125] S3. The nonwoven fabric obtained above is rolled up on a roll-forming machine and cut online to obtain a finished meltblown nonwoven material.

[0126] The test results of the obtained biodegradable melt-blown nonwoven fabric weight, filtration resistance, filtration efficiency, tensile strength, tensile elongation at break and average fiber diameter are shown in Table 3.

[0127] Comparative Example 4:

[0128] Prepare the materials and components according to the ratio in Table 2 and proceed as follows:

[0129] S1. Prepare mixed materials:

[0130] S11, drying the biodegradable resin PBAT at 80° C. for 14 h, and drying the PLA at 110° C. for 14 h to obtain a dry biodegradable material;

[0131] S12, stirring and uniformly mixing the biodegradable resin PBAT, PLA, and antioxidant in a high-speed mixer according to the formula ratio to obtain a mixed material;

[0132] S2, twin-screw granulation of the mixed material: the same conditions as in Example 2;

[0133] S3, preparing a melt-blown nonwoven fabric from the biodegradable PBAT / PLA blend slices prepared above: the same conditions as in Example 2;

[0134] S33, the nonwoven fabric obtained above is rolled up on a roll-forming machine and cut online to obtain a finished meltblown nonwoven material.

[0135] The biodegradable melt-blown nonwoven fabric obtained (such as Figure 4 ) The test results of gram weight, filtration resistance, filtration efficiency, tensile strength, tensile elongation at break and average fiber diameter are shown in Table 3.

[0136] Comparative Example 5:

[0137] Prepare the materials and components according to the ratio in Table 1 and proceed as follows:

[0138] S1, prepare mixed materials, same as in Example 1;

[0139] S2. The mixed material is subjected to twin-screw granulation, as in Example 1;.

[0140] S3, preparing melt-blown nonwoven fabric from the biodegradable PBAT / PLA blend slices prepared above:

[0141] S31, drying the biodegradable PBAT / PLA blended slices prepared above at 85° C. for 12 h.

[0142] S32, melt-blowing process: add the dried biodegradable PBAT / PLA blended slices into the automatic hopper of the melt-blowing device, send them into the screw extruder for heating and melting, the screw temperature is 170℃ in zone 1, 190℃ in zone 2, 220℃ in zone 3, 235℃ in zones 4-7, then the melt flows into the pre-filter to filter out impurities in the melt, and then flows to the metering pump with a flow rate of 8rpm. The melt is pressed out to the small orifice of the spinneret die (die temperature 230℃) by the pressure of the metering pump, and the spinneret is formed. The hole diameter is 0.28mm. The high-speed hot compressed air (245℃) on both sides of the small hole will perform hot air high-speed drawing on the melt extruded from the spinneret to obtain melt-blown ultrafine fibers. The fibers are cooled and crystallized in a short time. The side blowing fan speed is 1600rpm, and the suction fan speed under the net is 2100rpm. The fibers gather on the mesh curtain, the receiving distance DCD is 160mm, and the round net speed is 6m / mim, forming an ultrafine fiber melt-blown nonwoven fabric with good mechanical properties.

[0143] S33, the nonwoven fabric obtained above is rolled up on a roll-forming machine and cut online to obtain a finished meltblown nonwoven material.

[0144] The test results of the obtained biodegradable melt-blown nonwoven fabric weight, filtration resistance, filtration efficiency, tensile strength, tensile elongation at break and average fiber diameter are shown in Table 3.

[0145] Table 1 Examples and composition ratios of each group and meltblowing process

[0146] project Example 1 Example 2 Example 3 Example 4 Example 5 Biodegradable resin 90(PBAT) 75(PBAT) 60(PBAT) 90(PBS) 75(PBS) Polylactic acid (PLA) 10 25 40 10 25 Polypropylene 0 0 0 0 0 Tourmaline powder 0 0 0 0 0 Compatibilizer (maleic anhydride) 0.2 0.2 0.2 0.2 0.2 Lubricant (magnesium stearate) 0.1 0.1 0.1 0.1 0.1 Chain Extender (ADR4370S) 0.1 0.1 0.1 0.1 0.1 Antioxidant 168 0.1 0.1 0.1 0.1 0.1 Antioxidant 1010 0.1 0.1 0.1 0.1 0.1 Electrostatic charge (kV) 0 0 0 0 0

[0147] Table 2 Comparative Example Distribution Ratio Table and Meltblown Process

[0148] project Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Biodegradable resin 0 100(PBAT) 0 75(PBAT) 90(PBAT) Polylactic acid (PLA) 0 0 100 25 10 Polypropylene 97 0 0 0 0 Tourmaline powder 2 0 0 0 0 Maleic anhydride 0 0 0 0 0.2 Magnesium Stearate 1 0 0 0 0.1 ADR4370S 0 0 0 0 0.1 Antioxidant 168 0.1 0 0 0.1 0.1 Antioxidant 1010 0.1 0 0 0.1 0.1 Electrostatic charge (kV) 30 0 0 0 0

[0149] Through the test performance results of Examples 1-5, Comparative Example 1 and Table 3, it can be seen that the biodegradable melt-blown nonwoven fabric obtained by the formula and preparation method provided by the present invention, compared with the polypropylene melt-blown nonwoven fabric prepared by the conventional method, does not need to be subjected to electret treatment by an electrode device, which greatly saves energy consumption, and has better filtering performance and mechanical properties, and at the same time has a finer and more uniform fiber structure.

[0150] Through the test performance results of Examples 1-3 and Comparative Examples 2-4 and Table 3, it can be seen that only one biodegradable raw material (such as PBAT resin or PLA resin) is applicable, and the beneficial effects shown in the embodiments of the present invention cannot be obtained. In addition, when the compounded lubricant and dispersant are not added to the raw material formula, the beneficial effects shown in the embodiments of the present invention cannot be obtained. Adding compounded lubricants and dispersants plays a role in promoting crystallization and flow, and at the same time solves the system compatibility problem, making the material more stable. It is conducive to obtaining a melt-blown nonwoven material with excellent filtration performance and mechanical properties.

[0151] Through the test performance results of Example 1, Comparative Example 5 and Table 3, it can be seen that the formula is fixed, and the melt-blown process parameters (melt-blown nonwoven material preparation method) under the optimal conditions are changed and adjusted, and the beneficial effects shown in the embodiments of the present invention cannot be obtained. Therefore, the preparation method of the melt-blown nonwoven material provided by the present invention is conducive to obtaining a melt-blown nonwoven material with excellent filtration performance and mechanical properties.

[0152] At the same time, we can see from Table 3 that the biodegradable melt-blown nonwoven fabric obtained by blending PBAT and PLA in the present invention has a filtration efficiency of ≥97.5% and a ventilation resistance of ≤10.2, which are better than the melt-blown fabric made of polypropylene plus electret and electrostatic electret, and its transverse and longitudinal strength are better than polypropylene melt-blown fabric, and the longitudinal elongation of the embodiment is above 72.5%. Compared with polypropylene melt-blown fabric, the biodegradable melt-blown nonwoven fabric prepared by the present invention has excellent filtration performance, good elasticity, softer hand feel, and has a wider range of applications. Moreover, it can be seen from Comparative Examples 2 and 3 that the filtration efficiency of melt-blown fabrics prepared by PBAT and PLA alone is not good. PLA melt-blown fabric is relatively brittle (very low elongation) and has poor mechanical properties. By blending PBAT and PLA and optimizing the melt-blown process, a melt-blown nonwoven material with excellent filtration performance and good mechanical properties is obtained.

[0153] from Figure 1 to Figure 4 Compared with the meltblown cloth made of polypropylene plus electret, Example 2 prepared by the present invention has a finer and more uniform fiber structure, while the meltblown cloth made of PBAT alone has a coarse and uneven fiber diameter, and the meltblown cloth made of PLA alone has a fine fiber diameter but is extremely uneven, which also explains the differences in various performance indicators of the meltblown nonwoven materials in the above embodiments and comparative examples.

[0154] In addition, by adding a compatibilizer and a lubricant to the formula provided by the present invention, PBAT and PLA are blended more uniformly and have better compatibility. Figure 5As shown in the table, the compatibility of PBAT and PLA in Example 2 is significantly improved by optimizing the material formula. When observing the slice cross section, there are no holes in the blended slice after formula optimization, and the cut section is smooth and flat, which provides favorable conditions for the subsequent melt-blown process and makes it possible to produce melt-blown nonwoven products with excellent performance.

[0155]

Claims

1. A biodegradable meltblown nonwoven fabric material, Features: The material consists of the following components: The compatibilizer is maleic anhydride, and the chain extender is ADR4370S; The biodegradable resin is at least one of PBAT, PBST, PBSA and PBS; The lubricant is selected from at least one of zinc stearate, calcium stearate, and magnesium stearate and is mixed with the chain extender ADR4370S at a ratio of 1:0.5-1.5; the antioxidant is antioxidant 168 and antioxidant 1010 mixed at a ratio of 1:0.5-1.

5.

2. The biodegradable meltblown nonwoven material according to claim 1, Features:

3. The biodegradable meltblown nonwoven material according to claim 1 or 2, Features: The melt index of the biodegradable resin is 100-500 g / 10 min at 210° C. and 2.16 kg.

4. The biodegradable meltblown nonwoven material according to claim 3, Features: The melt index of the biodegradable resin is 300-500 g / 10 min at 210° C. and 2.16 kg.

5. The biodegradable meltblown nonwoven material according to claim 1, Features: The melt index of the polylactic acid is 80-400 g / 10 min at 250° C. and 2.16 kg.

6. The biodegradable meltblown nonwoven material according to claim 5, Features: The melt index of the polylactic acid is 50-400 g / 10 min at 250° C. and 2.16 kg; the molecular weight of the polylactic acid is between 100,000 and 130,000, and the melting point is 160° C.-170° C.

7. A method for preparing the biodegradable meltblown nonwoven fabric material according to claim 1, Features: The method comprises the following steps: S1. Prepare mixed materials: S11, stirring and mixing the dried biodegradable resin, polylactic acid, compatibilizer, lubricant, chain extender, and antioxidant in a high-speed mixer according to a formula ratio to obtain a mixed material; S2, twin-screw granulation of the mixed material: The mixed material is melted, extruded, air-cooled, drawn, and cold-cut to produce biodegradable resin / PLA blended biodegradable slices; S3, preparing melt-blown nonwoven fabric from the biodegradable resin / PLA blended biodegradable slices prepared above: S31, drying the biodegradable resin / PLA blended biodegradable slices prepared above at 70-90° C. for 6-24 hours; S32, melt-blown process: add the dried biodegradable resin / PLA blended biodegradable slices into the automatic hopper of the melt-blown device, send them into the screw extruder for heating and melting, flow into the pre-filter, filter out impurities in the melt, and then flow to the metering pump. The melt is pressed out to the small orifice of the spinneret die by the pressure of the metering pump. The diameter of the spinneret hole is 0.2-0.5mm. The high-speed hot compressed air on both sides of the small hole will perform hot air high-speed drawing on the melt extruded from the spinneret. The obtained melt-blown ultrafine fibers are cooled and crystallized in a short time under the action of side-blown cold wind. The fibers gather on the mesh curtain with a distance DCD of 160-250mm from the die head, wherein: the suction wind speed under the mesh is 1000-3000rpm; at the same time, the rotary screen runs at a speed of 3-10m / min, and is wound at a speed of 3-10m / min to form a melt-blown nonwoven fabric with ultrafine fibers; S33, the nonwoven fabric obtained above does not need to be subjected to electret treatment by an electrode device, and is finally rolled up on a roll-forming machine and slit online to obtain a finished meltblown nonwoven material.

8. The method for preparing the biodegradable meltblown nonwoven fabric material according to claim 7, Features: The method comprises the following steps: S1. Prepare mixed materials: S11, stirring and mixing the dried biodegradable resin, polylactic acid, compatibilizer, lubricant, chain extender, and antioxidant in a high-speed mixer according to a formula ratio to obtain a mixed material; S2, twin-screw granulation of the mixed material: Twin-screw granulation process: the mixed material obtained above is added through the silo and stirred continuously, the granulation screw temperature is 180-230°C, the screw speed is 200-300r / min, and the metering pump speed is 100-300kg / h; the mixed material is extruded, air-cooled, stretched, and cold-cut to make biodegradable resin / PLA blended biodegradable slices; S3, preparing melt-blown nonwoven fabric from the biodegradable resin / PLA blended biodegradable slices prepared above: S31, drying the biodegradable resin / PLA blended biodegradable slices prepared above at 70-90° C. for 6-24 hours; S32, melt-blown process: add the dried biodegradable resin / PLA blended biodegradable slices into the automatic hopper of the melt-blown device, send them into the screw extruder for heating and melting, flow into the pre-filter, filter out impurities in the melt, and then flow to the metering pump. The melt is pressed out to the small orifice of the spinneret die by the pressure of the metering pump. The diameter of the spinneret hole is 0.2-0.5mm. The high-speed hot compressed air on both sides of the small hole will perform hot air high-speed drawing on the melt extruded from the spinneret. The obtained melt-blown ultrafine fibers are cooled and crystallized in a short time under the action of side-blown cold wind. The fibers gather on the mesh curtain with a distance DCD of 160-250mm from the die head, wherein: the suction wind speed under the mesh is 1000-3000rpm; at the same time, the rotary screen runs at a speed of 3-10m / min, and is wound at a speed of 3-10m / min to form a melt-blown nonwoven fabric with ultrafine fibers; S33, the nonwoven fabric obtained above does not need to be subjected to electret treatment by an electrode device, and is finally rolled up on a roll-forming machine and slit online to obtain a finished meltblown nonwoven material.

9. The preparation method according to claim 8, Features: In the S32, the parameters are set as follows:

Citation Information

Cited By

  • Preparation method of high-strength degradable bi-component spunbond non-woven fabric

    CN122610294A