Preparation method of copolymerized self-coloring aramid fiber and copolymerized self-coloring aramid fiber

By embedding dye molecules with aromatic diamine structure into the aromatic polyamide main chain, self-colored aramid fibers were prepared by low-temperature copolymerization, which solved the problems of dyeing aramid fibers and achieved rich color and fastness. High, environmentally friendly and efficient fiber production meets diverse application needs.

CN115821417BActive Publication Date: 2024-12-03CHINA PETROLEUM & CHEMICAL CORP +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111094465.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-09-17
Publication Date
2024-12-03
Estimated Expiration
2041-09-17

AI Technical Summary

Technical Problem

The prior art has problems in the dyeing process of aramid fibers, low color rate, single color, low color fastness and mechanical strength decrease after high temperature treatment, which is difficult to meet the needs of diversified colors and small batch production. Commonly used dyeing methods have problems of environmental protection and high cost.

Method used

Through the copolymerization method, dye molecules with aromatic diamine structure are embedded into the main chain of aromatic polyamide macromolecules, and colored aramid fibers are prepared by low-temperature copolymerization method, and the monomer structure is controlled to regulate color development performance in a directional manner. The dryness is used. Spinning by wet spraying method, obtaining self-colored aramid fibers with rich colors, high color fastness, environmental protection, high efficiency and low cost.

Benefits of technology

It has achieved the improvement of color development, mechanical properties and thermal stability of aramid fibers, and has broken through the key technologies of industrial production of self-colored fibers. It has met the production requirements of high color fastness, environmental protection, high efficiency, short process and low cost, and expanded the production requirements of Its application requirements in various fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115821417B_ABST
    Figure CN115821417B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing a copolymerized self-coloring aramid and a copolymerized self-coloring aramid fiber. The preparation method comprises: adding anhydrous N-methylpyrrolidone and anhydrous calcium chloride to a reaction vessel, and after dissolving, adding p-phenylenediamine, aromatic diamine dye molecules and an acid binding agent; after stirring and dissolving, adding terephthaloyl chloride to react at a low temperature, and then heating the reaction when a pole climbing phenomenon occurs, so as to obtain the copolymerized self-coloring aramid. The present invention embeds a monomer with a coloring function into the main chain of an aromatic polyamide macromolecule by a copolymerization method, and prepares a self-coloring aramid fiber with excellent color development performance, mechanical properties and thermal stability by studying a spinning process. The present invention breaks through the key technology of the industrial production of self-coloring aramid fibers, meets the production requirements of high color fastness, environmental protection, high efficiency, short process and low cost, and broadens its application needs in various fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of aramid fiber preparation, and in particular to a preparation method of copolymerized self-coloring aramid and the copolymerized self-coloring aramid fiber. Background Art

[0002] As a new type of high-tech synthetic fiber, aramid fiber has excellent properties such as high strength, high modulus, high temperature resistance, acid and alkali resistance, etc. It has broad application prospects in national defense, aerospace, rail transportation, personal protection, information technology and new energy materials. However, aramid fiber has a compact molecular structure, high glass transition temperature and crystallinity. Conventional dyeing methods are prone to problems such as difficulty in dyeing and low coloring rate in the process of processing aramid fiber, resulting in difficulty in dyeing and single color of the product, which greatly limits the expansion of aramid fiber in the field of civil textiles with diversified color requirements. In previous studies, a lot of exploration has been carried out on the improvement of the dyeing performance of aramid fiber. Currently, the commonly used dyeing methods include solution dyeing, carrier dyeing, supercritical CO2 dyeing, etc. The solution dyeing method is the main dyeing method currently used for commercial aramid fiber in China. Without going through the dyeing process, the dye is directly added before the spinning of meta-aramid, and then the colored aramid fiber is obtained through the spinning process. The aramid fiber produced by this method has low color brightness, large color restrictions, low color fastness, and cannot be dyed after weaving, which makes it difficult to flexibly respond to customer demand for color and small batch production requirements. The carrier dyeing method is a dyeing method carried out in the dye liquor. Under high temperature conditions, the swelling degree of the aramid fiber is increased by the carrier effect in the dye liquor, and the diffusion rate of the dye inside the aramid fiber is accelerated, thereby increasing the absorption of the dye by the aramid fiber and improving the dyeing depth. However, after high temperature treatment, the crystallinity and orientation of the aramid fiber will decrease to varying degrees, and the mechanical strength will decrease. Secondly, the carrier itself has a strong irritating odor. The residual carrier after fabric dyeing is difficult to remove, which causes great pollution to people and the ecological environment. The supercritical CO2 dyeing method is a new type of non-aqueous medium dyeing and finishing technology. It does not require cleaning and drying operations, and the unused dyes, finishing agents and dyeing media can be recycled and reused. It overcomes the main shortcomings of water medium dyeing and finishing technology and makes the clean dyeing process of aramid fibers possible. However, during the dyeing process, dyes are greatly affected by temperature, pressure, molecular weight and molecular polarization. Secondly, dyeing and finishing equipment is complex and the cost investment is high. Therefore, there is still some distance to go in terms of large-scale production.

[0003] The prior art is to introduce dye molecules into the molecular chain through copolymerization to prepare colored polyimide, polyester and other copolymers, and further spin them to obtain self-coloring fibers. However, due to the limitations of aramid raw materials and structure, there are many problems in introducing dye molecules into aramid molecular chains, and it is difficult to prepare self-coloring aramid suitable for spinning, and further obtain aramid fibers with good wearability.

[0004] In view of this, it is necessary to design an improved preparation method of copolymerized self-coloring aramid and copolymerized self-coloring aramid fiber to solve the above problems. Summary of the invention

[0005] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide a method for preparing copolymerized self-coloring aramid and copolymerized self-coloring aramid fibers. Different chromophoric monomers with aromatic diamine structures are embedded into the main chain of aromatic polyamide macromolecules by copolymerization, and self-coloring aramid fibers with different colors are prepared by studying the spinning process, so that they have excellent color rendering properties, mechanical properties and thermal stability.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A method for preparing copolymerized self-coloring aramid fiber comprises the following steps:

[0008] S1. N-methylpyrrolidone and calcium chloride were added to the reaction vessel and stirred to completely dissolve the anhydrous calcium chloride;

[0009] S2. Under nitrogen protection, continue to add p-phenylenediamine, aromatic diamine dye molecules and acid binding agent to the reaction vessel, stirring to completely dissolve; wherein the concentration of p-phenylenediamine is 0.25 mol / L to 0.45 mol / L, and the molar ratio of the aromatic diamine dye molecules to the p-phenylenediamine is 1:60 to 1:10;

[0010] S3. The temperature of the reaction system is lowered to -5°C to 0°C, and the molar ratio of terephthaloyl chloride to the p-phenylenediamine is 1.03:1 to 1.15:1, terephthaloyl chloride is weighed and added to the reaction vessel, stirred and reacted;

[0011] S4. When the viscosity of the reaction system gradually increases and the pole climbing phenomenon occurs, the temperature of the reaction system is raised to 30-50° C., and stirring is continued to react to form a gel-like solid. The gel-like solid is washed, dried, and crushed to obtain the copolymer self-coloring aramid.

[0012] In the technical solution of the present invention, in step S3, the terephthaloyl chloride is divided into two equal parts and added into the reaction container successively, with an interval time of 15min to 30min in between and a stirring speed of 300 to 500r / min.

[0013] In the technical solution of the present invention, in step S1, the mass fraction of the anhydrous calcium chloride to the anhydrous N-methylpyrrolidone is 4% to 12%.

[0014] In the technical solution of the present invention, in step S1, the stirring and dissolving temperature of the anhydrous calcium chloride is 40-70°C, and after the calcium chloride is completely dissolved, the reaction system is cooled to 20-30°C.

[0015] In the technical solution of the present invention, in step S2, the molar ratio of the acid binding agent to the terephthaloyl chloride is 0.95:1 to 1.10:1.

[0016] In the technical solution of the present invention, in step S2, the acid binding agent is one or more of calcium hydride, pyridine, 2-methylpyridine, and calcium hydroxide.

[0017] In the technical scheme of the present invention, in step S2, the aromatic diamine dye molecules are one or more of 2,4-diaminoazobenzene-4-sulfonic acid, 2,4-diaminoazobenzene-2-sulfonic acid, 2,5-diaminoazobenzene-4-sulfonic acid, 2,5-diaminoazobenzene-2-sulfonic acid, 1,4-diaminoanthraquinone, 1,5-diaminoanthraquinone, 1,4-bis((4-aminophenyl)amino)anthracene-9,10-dione, 1,4-bis((2-methyl-4-aminophenyl)amino)anthracene-9,10-dione, 1,5-bis((4-aminophenyl)amino)anthracene-9,10-dione, and 1,5-bis((2-methyl-4-aminophenyl)amino)anthracene-9,10-dione.

[0018] In some specific technical solutions: the aromatic diamine dye molecule is at least one of the compounds prepared by the reaction routes shown in the following (1) to (4):

[0019]

[0020] The preparation method of the aromatic diamine dye molecule shown in formula (1) is:

[0021] Suspend p-aminobenzenesulfonic acid (17.3 g) in hydrochloric acid solution (300 mL, 1.0 M), and cool the solution in a water-ice bath at 0-5°C to obtain a mixed solution; dissolve sodium nitrite (7.25 g) in 50 mL of water under stirring to prepare solution A. Slowly add solution A to the mixed solution. After the nitrite solution is added, continue stirring at low temperature for 45-60 minutes to obtain a diazonium salt suspension;

[0022] Then, sodium carbonate (53.0 g) and p-phenylenediamine (11.3 g) were dissolved in 500 mL of water to prepare solution B, and the solution was cooled in a water-ice bath at 0-5°C. The diazonium salt suspension prepared in the previous step was slowly added dropwise to solution B with stirring. After the addition, the reaction was continued at 0-5°C for 60 min, and then dilute hydrochloric acid (1.0 M) was added to adjust the pH of the reaction system to neutral to form a large amount of precipitate. Filter and vacuum dry to obtain a red-black solid, which was recrystallized from ethanol-water to obtain the target product (2,5-diaminoazobenzene-4-sulfonic acid) with a purity of 98% and a yield of 75%. Figure 8 .

[0023] The preparation method of the aromatic diamine dye molecule shown in formula (2) is as follows: other conditions are the same as those of formula (1), except that p-aminobenzenesulfonic acid is replaced by o-aminobenzenesulfonic acid, and the yield of the target product (2,5-diaminoazobenzene-2-sulfonic acid) is 81% and the purity is 98%. Figure 7 .

[0024] The preparation method of the aromatic diamine dye molecule shown in formula (3) is as follows: other conditions are the same as those of formula (1), except that p-phenylenediamine is replaced by m-phenylenediamine. The yield of the target product (2,4-diaminoazobenzene-4-sulfonic acid) is 86% and the purity is 98%. Figure 5 .

[0025] The preparation method of the aromatic diamine dye molecule shown in formula (4) is as follows: other conditions are the same as those of formula (3), except that p-aminobenzenesulfonic acid is replaced by o-aminobenzenesulfonic acid, and the yield of the target product (2,4-diaminoazobenzene-2-sulfonic acid) is 85% and the purity is 98%. Figure 6 .

[0026] In some other specific technical solutions: the aromatic diamine dye molecule is a compound prepared by the reaction route shown in the following formula (5):

[0027]

[0028] The preparation method of the aromatic diamine dye molecule shown in formula (5) is:

[0029] In a 250mL flask, weigh 1,4-dibromoanthraquinone compound (3.63g), palladium acetate (70mg), Xantphos (160mg), potassium tert-butoxide (3.36g) and Boc mono-protected 2,5-diaminotoluene (3.33g) and add. Under nitrogen protection, add 175mL of 1,4-dioxane and place in an 80℃ oil bath for reflux reaction for 12h. Thin layer chromatography is used to detect the progress of the reaction. After the reaction is completed, the solvent 1,4-dioxane is dried, and then 200mL of dichloromethane is added to dissolve. The solution is washed three times with 50mL of water, and the solvent is dried to obtain a crude product. The obtained crude product was dissolved in 50 mL of 4M HCl 1,4-dioxane solution, stirred at room temperature for 4 h, and the reaction progress was detected by thin layer chromatography. After the reaction was completed, the solvent was dried, and then 200 mL of dichloromethane was added. The solution was washed three times with 50 mL of NaOH solution (1 M). The organic phase was dried over anhydrous NaSO4 and separated by column chromatography (MeOH:DCM=1:20) to obtain the target compound (1,4-bis((2-methyl-4-aminophenyl)amino)anthracene-9,10-dione), such as Fig. 9 The yield was 80% and the purity was 98%.

[0030] In some other specific technical solutions: the aromatic diamine dye molecule is a compound prepared by the reaction route shown in the following formula (6):

[0031]

[0032] In a 250 mL flask, weigh 1,5-dichloroanthraquinone compound (2.75 g), palladium acetate (70 mg), Xantphos (160 mg), potassium tert-butoxide (3.36 g) and Boc mono-protected 2,5-diaminotoluene (3.33 g) and add. Under nitrogen protection, add 175 mL of 1,4-dioxane and place in an 80 ° C oil bath for reflux reaction for 12 hours. Thin layer chromatography is used to detect the progress of the reaction. After the reaction is completed, the solvent 1,4-dioxane is dried, and then 200 mL of dichloromethane is added to dissolve. The solution is washed three times with 50 mL of water, and the solvent is dried to obtain a crude product. The obtained crude product was dissolved in 50 mL of 4M HCl 1,4-dioxane solution, and the mixture was stirred at room temperature for 4 h. The reaction progress was detected by thin layer chromatography. After the reaction was completed, the solvent was dried, and then 200 mL of dichloromethane was added. The solution was washed three times with 50 mL of NaOH solution (1 M). The organic phase was dried over anhydrous NaSO4 and separated by column chromatography (MeOH:DCM=1:20) to obtain the target compound (1,5-bis((2-methyl-4-aminophenyl)amino)anthracene-9,10-dione) with a yield of 83% and a purity of 98%. Fig.10 .

[0033] The following formula gives a synthetic route for copolymerization of aromatic diamine dye molecules to produce self-colored aramid (PPTA-R):

[0034] In summary, the present invention embeds dye molecules with aromatic diamine structures into the main chain of aromatic polyamide molecules through a step-by-step low-temperature copolymerization method to prepare self-coloring aromatic polyamide, and directionally regulates the color rendering properties of aromatic polyamide by controlling the monomer structure. The aramid fiber prepared by this method has rich and uniform colors, high color fastness, environmental protection, high efficiency, low cost and simple operation. A copolymer self-coloring aramid fiber is obtained by spinning the copolymer self-coloring aramid prepared by the above preparation method.

[0035] In some specific technical solutions, the spinning method of the copolymerized self-colored aramid fiber adopts dry-jet wet spinning, and the concentration of the spinning solution is 15%-22%.

[0036] In some specific technical solutions, the copolymerized self-coloring aramid fiber has a strength of 15-30 cN / dtex, an elastic modulus of 60-100 GPa, and color fastness: color fastness to soaping reaches level 3-4 according to GB / T3921-2008 standard, color fastness to friction reaches level 3-4 according to GB / T3920 standard, and color fastness to perspiration reaches level 3-4 according to GB / T3922 standard. Beneficial effects of the present invention:

[0037] 1. The method for preparing the copolymerized self-coloring aramid provided by the present invention is to embed different chromophoric monomers with aromatic diamine structures into the main chain of aromatic polyamide macromolecules according to the requirements of different application fields for the color and performance of aramid fibers, thereby preparing self-coloring aromatic polyamide, and to directionally regulate the color rendering properties of aromatic polyamide by controlling the monomer structure. By studying the spinning process, self-coloring aramid fibers with different colors are prepared, which have excellent color rendering properties, mechanical properties and thermal stability, and the relationship between the structure and performance of self-coloring aramid fibers is established. The key technology of industrial production of self-coloring aramid fibers has been broken through, and the production requirements of high color fastness, environmental protection, high efficiency, short process and low cost can be met, which significantly broadens its application needs in various fields.

[0038] 2. The method for preparing the copolymerized self-coloring aramid provided by the present invention is to embed dye molecules with an aromatic diamine structure into the main chain of the aromatic polyamide molecule by a step-by-step low-temperature copolymerization method to prepare the self-coloring aromatic polyamide. The aramid fiber prepared by the method has rich and uniform colors and high color fastness, and has the advantages of environmental protection, high efficiency, low cost, and simple operation, and is suitable for industrial production.

[0039] 3. The method for preparing the copolymerized self-coloring aramid provided by the present invention is oriented to control the preparation method of the copolymerized self-coloring aramid based on the color development and mechanical wearability of the aramid fiber. The method mainly controls the solvent content, i.e., the raw material concentration in the reaction solution, and the content of the aromatic diamine dye molecules to prepare the self-coloring aramid suitable for spinning. The self-coloring aramid fiber with good color uniformity, high durability and high strength can be obtained by spinning the self-coloring aramid fiber, which has good wearability and broadens the large-scale application of aramid fiber. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 From left to right in the figure are the colors of 1,5-diaminoanthraquinone, 1,5-bis((4-aminophenyl)amino)anthracene-9,10-dione, and 1,4-bis((4-aminophenyl)amino)anthracene-9,10-dione solutions.

[0041] Figure 2 From left to right in the figure are the actual pictures of the original aramid 1414, the self-colored brown aramid prepared in Example 1, and the self-colored purple aramid prepared in Example 7.

[0042] Figure 3 This is the FTIR spectrum of the PPTA-R aramid fiber (R is 1,5-bis((4-aminophenyl)amino)anthracene-9,10-dione) prepared in Example 6.

[0043] Figure 4 This is the TG curve of the PPTA-R aramid fiber (R is 1,5-bis((4-aminophenyl)amino)anthracene-9,10-dione) prepared in Example 6.

[0044] Figure 5 This is the hydrogen nuclear magnetic resonance spectrum of the target product (2,4-diaminoazobenzene-4-sulfonic acid).

[0045] Figure 6 This is the hydrogen nuclear magnetic resonance spectrum of the target product (2,4-diaminoazobenzene-2-sulfonic acid).

[0046] Figure 7 This is the hydrogen nuclear magnetic resonance spectrum of the target product (2,5-diaminoazobenzene-2-sulfonic acid).

[0047] Figure 8 This is the hydrogen nuclear magnetic resonance spectrum of the target product (2,5-diaminoazobenzene-4-sulfonic acid).

[0048] Fig. 9 This is the spectrum of the target compound (1,4-bis((2-methyl-4-aminophenyl)amino)anthracene-9,10-dione).

[0049] Fig.10This is the spectrum of the target compound (1,5-bis((2-methyl-4-aminophenyl)amino)anthracene-9,10-dione). DETAILED DESCRIPTION

[0050] The present invention is further described below in conjunction with embodiments, but the protection scope of the present invention is not limited thereto:

[0051] The present invention is guided by the color development and mechanical and other wearing properties of aramid fibers, and directionally regulates the preparation method of copolymerized self-coloring aramid fibers, thereby preparing self-coloring aramid fibers suitable for spinning. By spinning the self-coloring aramid fibers, self-coloring aramid fibers with good color uniformity, high durability and high strength can be obtained, which meets the production requirements of high color fastness, environmental protection, high efficiency, short process and low cost, and broadens its application needs in various fields.

[0052] Examples 1-14 and Comparative Examples 1-4

[0053] A copolymer self-coloring aramid fiber is prepared by low-temperature copolymerization using terephthaloyl chloride (TPC), p-phenylenediamine (PPD) and aromatic diamine dye molecules as raw materials. The specific experimental steps are as follows:

[0054] Set up a mechanical stirring reaction device, first introduce nitrogen into the device to expel the air in the device, and the exhaust time is 13 minutes. Then add anhydrous N-methylpyrrolidone (NMP) and anhydrous calcium chloride (4%-12% by mass fraction of the solvent) into the reaction bottle, heat to 60°C and stir to dissolve (speed 100r / min).

[0055] After calcium chloride is completely dissolved, the reaction system is cooled to 25°C. Under nitrogen protection, p-phenylenediamine (concentration of the reaction system is 0.25mol / L to 0.45mol / L), aromatic diamine dye molecules (the ratio of the amount of p-phenylenediamine substance is 1:60 to 1:10) and pyridine (the ratio of the amount of terephthaloyl chloride substance is 0.95:1-1.10:1) are weighed and added to the reaction bottle, and stirring and dissolving are continued (150r / min). After the compound is completely dissolved, the reaction system is cooled to -5°C to 0°C.

[0056] Weigh terephthaloyl chloride (with a molar ratio of 1.03:1 to 1.15:1 to p-phenylenediamine), divide it into two equal parts and add them to the reaction system successively, with an interval of 18 minutes in between and the stirring speed is 470r / min. After the addition of terephthaloyl chloride, continue stirring for 30 minutes. It is clearly observed that the viscosity of the reaction system gradually increases, and the climbing phenomenon occurs. Then gradually heat up to 40°C, continue stirring for 2 hours, and a gel-like solid is formed. The solid is washed with a large amount of water to neutrality, crushed into powder by a pulverizer, washed with a large amount of ethanol to remove small molecules, and dried to obtain self-colored aramid.

[0057] Comparative Example 5

[0058] Add 500mL of N,N-dimethylacetamide to the reactor, then add 6g of polyvinylpyridine dispersant and stir evenly. Then add 10.26g of p-phenylenediamine, 1.19g of 1,4-diaminoanthraquinone and 23.7g of pyridine and continue to stir evenly. After cooling the reaction system to 5°C, weigh 20.3g of terephthaloyl chloride and add it to the reaction system. Stir the reaction for 2h. After the reaction is completed, centrifuge and wash with water three times to obtain aramid ultrafine fibers.

[0059] Table 1 Preparation conditions of Examples 1-9 and Comparative Examples 1-4

[0060]

[0061]

[0062]

[0063] The copolymerized self-colored aramid prepared in the above Examples 1-9 and Comparative Examples 1-4 was spun: PPTA-R was dissolved in 100% H2SO4 to prepare a spinning solution with a concentration of 15%-20%, and then the spinning was carried out by dry-jet wet spinning.

[0064] Table 2 Performance test results of fibers prepared in Examples 1-9 and Comparative Examples 1-4

[0065]

[0066]

[0067] The properties of the obtained copolymer self-coloring aramid fiber are shown in Table 2. It can be seen that when the mass fraction of CaCl2 is 8%, the obtained aramid has higher strength and high color fastness; when the mass fraction of CaCl2 is too high or too low, the obtained aramid strength decreases and the color fastness decreases. When the concentration of p-phenylenediamine is between 0.25mol / L and 0.45mol / L, the obtained aramid has higher strength. When the concentration of p-phenylenediamine is too high or too low, the obtained aramid strength decreases and the color fastness decreases. When the amount of aromatic diamine dye molecules added increases, the strength of the obtained aramid decreases. When the amount of pyridine added is appropriate (the molar ratio with terephthaloyl chloride is 0.95:1-1.10:1), the obtained aramid has higher strength and high color fastness.

[0068] In summary, the preparation method of the copolymerized self-coloring aramid provided by the present invention embeds dye molecules with an aromatic diamine structure into the main chain of the aromatic polyamide molecule by a step-by-step low-temperature copolymerization method to prepare a self-coloring aromatic polyamide. And the preparation method of the copolymerized self-coloring aramid is directional regulated with the color development and mechanical and other wear properties of the aramid fiber as the guide. Thus, a self-coloring aramid suitable for spinning is prepared, and it is spun to obtain a self-coloring aramid fiber with good color uniformity, high durability and high strength, and good wear properties, which broadens the large-scale application of aramid fibers. The above embodiments are only used to illustrate the technical scheme of the present invention and are not limited. Although the present invention is described in detail with reference to the preferred embodiments, ordinary technicians in the field should understand that the technical scheme of the present invention can be modified or equivalently replaced without departing from the spirit and scope of the technical scheme of the present invention.

Claims

1. A copolymer self-coloring aramid fiber, characterized in that: The copolymerized self-coloring aramid fiber is obtained by spinning copolymerized self-coloring aramid, and the molecular chain of the copolymerized self-coloring aramid includes aromatic diamine dye molecules and p-phenylenediamine in a molar ratio of 1:60 to 1:10; the copolymerized self-coloring aramid fiber has a strength of 15 to 30 cN / dtex, an elastic modulus of 60 to 100 GPa, and color fastness: color fastness to soaping reaches level 3 to 4, color fastness to friction reaches level 3 to 4, and color fastness to perspiration reaches level 3 to 4; The preparation method of the copolymerized self-coloring aramid fiber comprises the following steps: S1. Anhydrous N-methylpyrrolidone and anhydrous calcium chloride are added to the reaction vessel, and the anhydrous calcium chloride is stirred to completely dissolve; the mass fraction of the anhydrous calcium chloride in the anhydrous N-methylpyrrolidone is 4% to 12%; S2. Under nitrogen protection, p-phenylenediamine, aromatic diamine dye molecules and acid binding agent are added to the reaction vessel and stirred to completely dissolve; wherein the concentration of p-phenylenediamine is 0.25 mol / L ~ 0.45 mol / L, and the molar ratio of the aromatic diamine dye molecules to the p-phenylenediamine is 1:60 ~ 1:10; S3. The temperature of the reaction system is lowered to -5°C to 0°C, and the molar ratio of terephthaloyl chloride to the p-phenylenediamine is 1.03:1 to 1.15:1, terephthaloyl chloride is weighed and added to the reaction vessel, and the reaction is stirred for a preset time; S4. When the viscosity of the reaction system gradually increases and the pole climbing phenomenon occurs, the temperature of the reaction system is raised to 30-50° C., and the stirring reaction is continued for a preset time to form a gel-like solid, and the gel-like solid is washed, dried, and crushed to obtain the copolymer self-coloring aramid.

2. The copolymerized self-coloring aramid fiber according to claim 1, characterized in that: The aromatic diamine dye molecules are one or more of 2,4-diaminoazobenzene-4-sulfonic acid, 2,4-diaminoazobenzene-2-sulfonic acid, 2,5-diaminoazobenzene-4-sulfonic acid, 2,5-diaminoazobenzene-2-sulfonic acid, 1,4-diaminoanthraquinone, 1,5-diaminoanthraquinone, 1,4-bis((4-aminophenyl)amino)anthracene-9,10-dione, 1,4-bis((2-methyl-4-aminophenyl)amino)anthracene-9,10-dione, 1,5-bis((4-aminophenyl)amino)anthracene-9,10-dione, and 1,5-bis((2-methyl-4-aminophenyl)amino)anthracene-9,10-dione.

3. The copolymerized self-coloring aramid fiber according to claim 1, characterized in that: The spinning method of the copolymerized self-colored aramid fiber adopts a dry-jet wet spinning method, and the concentration of the spinning solution is 15% to 22%.

4. The copolymerized self-coloring aramid fiber according to claim 1, characterized in that: In step S3, the terephthaloyl chloride is divided into two equal parts and added into the reaction container successively, with an interval of 15 min to 30 min in between and a stirring speed of 300 to 500 r / min.

5. The copolymerized self-coloring aramid fiber according to claim 1, characterized in that: In step S1, the stirring and dissolving temperature of the anhydrous calcium chloride is 40-70°C. After the calcium chloride is completely dissolved, the reaction system is cooled to 20-30°C.

6. The copolymerized self-coloring aramid fiber according to claim 1, characterized in that: In step S2, the molar ratio of the acid binding agent to the terephthaloyl chloride in step S3 is 0.95:1 to 1.10:1; the acid binding agent is one or more of calcium hydride, pyridine, 2-methylpyridine, and calcium hydroxide.