A mica glass fiber composite material and its preparation method and application

By combining the mica layer and the resin fiberglass cloth layer, the mica fiberglass composite material solves the problem of insufficient mechanical strength and high temperature resistance of the existing mica board, achieves all-round protection and safety improvement at the bottom of the battery, and at the same time reduces the battery pack weight.

CN115831443BActive Publication Date: 2024-10-01GOODE EIS SUZHOU CORP LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211339040.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-28
Publication Date
2024-10-01
Estimated Expiration
2042-10-28

AI Technical Summary

Technical Problem

The existing mica plates have insufficient mechanical strength and high temperature resistance, and cannot effectively protect the battery pack from flame cascading and other mechanical damage caused by thermal runaway. The large thickness increases the weight of the battery pack, which is not conducive to installation and use.

Method used

A mica fiberglass composite material that combines a mica layer and a resin fiberglass cloth layer is used. By adjusting the material composition and stacking settings of the mica layer and resin fiberglass cloth, the impact resistance and high temperature resistance of the material are enhanced for battery bottom protection. , forming structural parts with thin thickness and light weight.

Benefits of technology

The high mechanical properties, fire retardant properties and high temperature resistance of the mica fiberglass composite material are achieved, which can effectively prevent flame cascading after the battery thermal runaway, mitigate potential safety hazards, and reduce the overall weight of the battery pack.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003915727050000101
    Figure BDA0003915727050000101
  • Figure BDA0003915727050000111
    Figure BDA0003915727050000111
Patent Text Reader

Abstract

The present invention discloses a mica glass fiber composite material and a preparation method and application thereof. The mica glass fiber composite material of the present invention comprises a mica layer and a resin glass fiber cloth layer connected to each other, wherein the mica layer comprises a mica material and an adhesive in a mass ratio of 100:(10-25), and the resin glass fiber cloth layer comprises a glass fiber cloth and a resin in a mass ratio of 100:(45-65). The mica glass fiber composite material of the present invention has thin thickness, light weight, good mechanical properties, high temperature resistance of 1200°C without deformation, good thermal insulation, strong impact resistance, and can be used for structural parts to protect the bottom of the battery, which can be more effective, all-round protection and delay of safety problems caused by thermal runaway of the battery pack.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of mica composite materials, and in particular to a mica glass fiber composite material and a preparation method and application thereof. Background Art

[0002] With the global shortage of oil resources and the intensification of the greenhouse effect, the development of new energy electric vehicles has become a general trend. Although new energy electric vehicles have been on the market for many years, battery safety issues still exist. Once the battery catches fire and gets out of control, it will instantly release high-temperature and high-pressure flames, endangering the safety of people in the car; at the same time, electric vehicles cause hot air flows due to problems such as battery thermal runaway, which can easily cause damage to all directions inside the battery pack and cause other units of the battery pack to burn, thereby causing damage to other parts of the car and operators. Therefore, generally, setting up protective devices outside the battery assembly can effectively protect and delay damage to operators and other parts.

[0003] However, in the prior art, the fireproof material used in such protective devices generally adopts a single mica board. The mica board is an insulating material made of mica paper and adhesive by heating and pressing. It is widely used in different fields such as new energy vehicles, household appliances and metallurgical industries. Although the mica board has excellent insulation properties, due to its low mechanical strength, the material is brittle and has poor impact resistance. When mechanical equipment such as motors runs at high speed for a long time, the mica board is prone to wear, which can easily affect the normal operation of mechanical equipment such as motors. Therefore, it can only protect the top of the battery and cannot bear too much weight. Its mechanical properties, fireproof properties and high temperature resistance need to be further improved.

[0004] CN114523741A discloses a high-strength, high-tensile, high-modulus mica board for thermal runaway management of new energy vehicles and its preparation method. The mica board includes a mica substrate and a modified glass fiber cloth, the modified glass fiber cloth is compounded on the surface of the mica substrate by a powder adhesive, and the modified glass fiber cloth includes a glass fiber base cloth and a silicon nitride film deposited on the surface of the glass fiber base cloth by plasma chemical vapor deposition; the preparation method includes the following steps: S1, spraying the powder adhesive evenly on the surface of the mica substrate and baking at 75-80°C for 4-7min; S2, compounding the modified glass fiber cloth on the side of the mica substrate sprayed with the powder adhesive, and hot pressing and shaping at 120-130°C for 30-40min to obtain a product, which has the advantage of improving the mechanical strength of the mica board. However, the mechanical properties and high temperature resistance of the material need to be further improved.

[0005] CN206564279U discloses a flame retardant fireproof heat insulation board, including a ceramic glue fireproof layer and an insulating heat insulation group. The ceramic glue fireproof layer is coated on the outside of the insulating heat insulation group, and the insulating heat insulation group includes one or more insulating heat insulation layers. When the insulating heat insulation group has a plurality of insulating heat insulation layers, the plurality of insulating heat insulation layers can be a combination of a plurality of layers of white carbon black, a plurality of layers of mica sheets, or a plurality of layers of white carbon black and mica sheets. The ceramic glue fireproof layer on the outside of the flame retardant fireproof heat insulation board of the utility model can be transformed into a ceramic-like hard shell to form a firewall when encountering fire, and the internal insulating heat insulation group can isolate the transfer of heat, so that the effects of fire prevention, flame retardancy and heat insulation can be achieved. When applied to a battery pack, it is avoided that the temperature of one of the batteries is too high and burns and is damaged, thereby ensuring the overall safety of the battery pack. However, the thick insulating heat insulation group causes the battery to be heavy, which is not conducive to the installation and use of the battery pack.

[0006] Therefore, it is necessary to develop a mica glass fiber composite material with thin thickness, good mechanical properties, high temperature resistance and impact resistance and a preparation method thereof. Summary of the invention

[0007] In view of the deficiencies in the prior art, the object of the present invention is to provide a mica glass fiber composite material and a preparation method and application thereof. The mica glass fiber composite material of the present invention has thin thickness, light weight, good mechanical properties, can withstand high temperatures of 1200°C without deformation, has good thermal insulation, and strong impact resistance. It can be used for structural parts to protect the bottom of the battery, and can more effectively and comprehensively protect and delay safety problems caused by thermal runaway of the battery pack.

[0008] One of the purposes of the present invention is to provide a mica glass fiber composite material. To achieve this purpose, the present invention adopts the following technical solutions:

[0009] A mica glass fiber composite material comprises a mica layer and a resin glass fiber cloth layer connected to each other, wherein the mica layer comprises a mica material and an adhesive in a mass ratio of 100:(10-25), and the resin glass fiber cloth layer comprises a glass fiber cloth and a resin in a mass ratio of 100:(45-65).

[0010] The mica glass fiber composite material of the present invention combines a mica layer with a resin glass fiber cloth layer, which effectively avoids the problem that the mica material alone is brittle and has poor impact resistance, resulting in the inability to use mica material for protection under the battery. By adjusting the material composition of the mica layer and the resin glass fiber cloth, the impact resistance of the material is effectively enhanced, and it can be used for structural parts to protect the bottom of the battery, effectively mitigating the safety hazard after thermal runaway of the battery.

[0011] In the present invention, the mica layer and the resin glass fiber cloth layer are stacked, and the total number of mica layers and resin glass fiber cloth layers can be 2-20 layers, such as 2 layers, 3 layers, 4 layers, 5 layers, 6 layers, 7 layers, 8 layers, 9 layers, 10 layers, 11 layers, 12 layers, 13 layers, 14 layers, 15 layers, 16 layers, 17 layers, 18 layers, 19 layers, 20 layers, etc., and can also be adjusted to more layers according to actual needs. The mica layer and the resin glass fiber cloth layer are stacked, for example, one mica layer and one resin glass fiber cloth layer can be stacked, It can also be two mica layers and one resin glass fiber cloth layer stacked, or it can be three mica layers and one resin glass fiber cloth layer stacked; it can also be one mica layer and two resin glass fiber cloth layers stacked, one mica layer and three resin glass fiber cloth layers stacked, two mica layers and two resin glass fiber cloth layers stacked, three mica layers and two resin glass fiber cloth layers stacked, etc.; preferably, in the total number of layers of the composite material, the ratio of mica layers to resin glass fiber cloth layers is (2-4):1, preferably 3:1.

[0012] In the present invention, the mica layer comprises a mica material and an adhesive in a mass ratio of 100:(10-25), for example, the mass ratio of the mica material and the adhesive is 100:10, 100:11, 100:12, 100:13, 100:14, 100:15, 100:16, 100:17, 100:18, 100:19, 100:20, 100:21, 100:22, 100:23, 100:24, 100:25, etc. If the mass ratio of the mica material and the adhesive is too low, lower than 100:10, the finished product will have poor adhesion and easy delamination; if the mass ratio of the mica material and the adhesive is too high, higher than 100:25, the material strength will be reduced.

[0013] In the present invention, the resin fiberglass cloth layer comprises fiberglass cloth and resin in a mass ratio of 100:(45-65), for example, the mass ratio of fiberglass cloth and resin is 100:45, 100:46, 100:47, 100:48, 100:49, 100:50, 100:51, 100:52, 100:53, 100:54, 100:55, 100:56, 100:57, 100:58, 100:59, 100:60, 100:61, 100:62, 100:63, 100:64 or 100:65, etc. If the mass ratio of fiberglass cloth and resin is too low, lower than 100:45, the finished product will have poor adhesion and easy delamination; if the mass ratio of fiberglass cloth and resin is too high, higher than 100:65, the material strength will be reduced.

[0014] The present invention adjusts the material composition of the mica layer and the resin glass fiber cloth so that the prepared fireproof material has strong mechanical properties, fire retardant properties and high temperature resistance. It can be used as a battery pack structural component to provide all-round protection for the battery, effectively prevent flame burning caused by thermal runaway of the battery, and thus effectively reduce the safety hazards after thermal runaway of the battery.

[0015] The mica material is phlogopite or muscovite.

[0016] The adhesive is any one of epoxy resin, silicone resin and phenolic resin or a mixture of at least two of them.

[0017] The resin is epoxy resin and / or silicone resin.

[0018] In the present invention, the glass fiber cloth is made by drawing glass into extremely fine glass filaments, and the glass filaments at this time have good softness. The glass filaments are spun into yarns, and then woven into glass fiber cloth through a loom, which is an inorganic non-metallic material with excellent performance. There are many types of glass fiber cloth, and the advantages are good insulation, strong heat resistance, good corrosion resistance, and high mechanical strength. Preferably, the main specifications of the glass fiber cloth are 7637, 7630, 7628, 7615, 1506, 2116, 2113, 3313, 1080, 106, 104, etc.

[0019] Specifically, the thickness of the glass fiber cloth is 0.05-0.07 mm, for example, 0.05 mm, 0.06 mm, 0.07 mm, etc.; the mesh number is 100-200 mesh, for example, 100 mesh, 110 mesh, 120 mesh, 130 mesh, 140 mesh, 150 mesh, 160 mesh, 170 mesh, 180 mesh, 190 mesh, 200 mesh, etc.

[0020] In the present invention, the thickness of the mica layer is 0.2 to 2 mm. For example, the thickness of the mica layer is 0.2 mm, 0.3 mm, 0.4 mm, 0.5 mm, 0.6 mm, 0.7 mm, 0.8 mm, 0.9 mm, 1 mm, 1.1 mm, 1.2 mm, 1.3 mm, 1.4 mm, 1.5 mm, 1.6 mm, 1.7 mm, 1.8 mm, 1.9 mm or 2 mm.

[0021] In the present invention, the thickness of the resin glass fiber cloth layer is 0.05-0.2 mm, for example, the thickness of the resin glass fiber cloth layer is 0.05 mm, 0.06 mm, 0.07 mm, 0.08 mm, 0.09 mm, 0.1 mm, 0.11 mm, 0.12 mm, 0.13 mm, 0.14 mm, 0.15 mm, 0.16 mm, 0.17 mm, 0.18 mm, 0.19 mm, 0.2 mm, etc.

[0022] By adjusting the thickness of the mica layer and the resin glass fiber cloth layer, the present invention can ensure that the mica layer and the resin glass fiber cloth layer have the minimum thickness while ensuring basic insulation and fireproof performance, while at the same time enhancing the mechanical strength and reducing the weight, so that they can be used for battery structural parts to provide all-round protection for battery components.

[0023] The second object of the present invention is to provide a method for preparing the mica glass fiber composite material described in the first object, comprising the following steps:

[0024] (1) preparing a mica layer material using a mica material and an adhesive as raw materials according to a ratio;

[0025] (2) preparing a resin glass fiber cloth layer material using glass fiber cloth and resin as raw materials according to a ratio;

[0026] (3) The mica layer material and the resin glass fiber cloth layer material are stacked and hot-pressed to obtain the mica glass fiber composite material.

[0027] Preferably, the hot pressing pressure is 500-800T, for example, 500T, 550T, 600T, 650T, 700T, 750T, 800T, etc.

[0028] Preferably, the hot pressing temperature is 115-130°C, for example, 115°C, 120°C, 125°C, 130°C, etc.; the hot pressing time is 10-30min, for example, 10min, 15min, 20min, 25min, 30min, etc.

[0029] As a preferred embodiment of the present invention, the method for preparing the mica glass fiber composite material comprises the following steps:

[0030] (1) Cut 300*300mm laminated mica paper and 300*300mm resin fiberglass cloth;

[0031] (2) stacking mica paper and resin glass fiber cloth in a multi-layer combination of mica paper, resin glass fiber cloth, mica paper, and resin glass fiber cloth;

[0032] (3) placing the stacked mica paper and resin glass fiber cloth composite sheets on a hot pressing device, and hot pressing and curing them at 115-130° C. for 10-30 minutes under a pressure of 500-800T to obtain a mica glass fiber composite material.

[0033] The third object of the present invention is to provide an application of the mica glass fiber composite material described in the first object, wherein the mica glass fiber composite material is used for the preparation of structural parts to protect the bottom of the battery, thereby effectively alleviating the safety hazards after thermal runaway of the battery.

[0034] Compared with the prior art, the present invention has the following beneficial effects:

[0035] The mica glass fiber composite material of the present invention is thin, light, has good mechanical properties, can withstand high temperatures of 1200°C without deformation, has good thermal insulation, and has strong impact resistance. It can be used for structural parts to protect the bottom of the battery, and can more effectively and comprehensively protect and delay safety problems caused by thermal runaway of the battery pack. Specifically, the tensile strength of the prepared mica glass fiber composite material is 178-235MPa, the bending strength is 303-350MPa, and the impact resistance is 28.8-36.7KJ / m 2 , the hot surface insulation performance test is 1000±200℃ and the cold surface temperature is 277-295℃. DETAILED DESCRIPTION

[0036] The technical solution of the present invention is further illustrated below through specific implementation methods.

[0037] Unless otherwise specified, various raw materials of the present invention can be purchased from the market or prepared according to conventional methods in the art.

[0038] Example 1

[0039] The mica glass fiber composite material of this embodiment comprises mica layers and resin glass fiber cloth layers connected to each other, with a total number of 16 layers, and the ratio of the number of layers of the mica layer to the resin glass fiber layer is 3:1. The mica layer comprises a mica material and an adhesive in a mass ratio of 100:18, the mica material is a natural mineral material of muscovite mica, and the adhesive is bisphenol A epoxy resin 128 epoxy resin; the resin glass fiber cloth layer comprises a glass fiber cloth and a resin in a mass ratio of 100:55, the glass fiber cloth is an alkali-free glass fiber, and the resin is bisphenol A epoxy resin 128 epoxy resin.

[0040] The preparation method of the mica glass fiber composite material of this embodiment comprises the following steps:

[0041] (1) Cut 300*300mm laminated mica paper and 300*300mm resin fiberglass cloth;

[0042] (2) stacking mica paper and resin glass fiber cloth in a multi-layer combination of mica paper, resin glass fiber cloth, mica paper, and resin glass fiber cloth;

[0043] (3) The stacked mica paper and resin glass fiber cloth composite sheets are placed on a hot pressing device, and hot-pressed and cured at 120° C. for 20 minutes under a pressure of 600T to obtain a mica glass fiber composite material.

[0044] Example 2

[0045] The mica glass fiber composite material of this embodiment comprises mica layers and resin glass fiber cloth layers connected to each other, with a total number of 16 layers, and the ratio of the number of layers of the mica layer to the resin glass fiber layer is 3:1. The mica layer comprises a mica material and an adhesive in a mass ratio of 100:15, the mica material is a natural mineral material of muscovite mica, and the adhesive is bisphenol A epoxy resin 128 epoxy resin; the resin glass fiber cloth layer comprises a glass fiber cloth and a resin in a mass ratio of 100:45, the glass fiber cloth is an alkali-free glass fiber, and the resin is bisphenol A epoxy resin 128 epoxy resin.

[0046] The preparation method of the mica glass fiber composite material of this embodiment is the same as that of Example 1.

[0047] Example 3

[0048] The mica glass fiber composite material of this embodiment comprises mica layers and resin glass fiber cloth layers connected to each other, with a total number of 16 layers, and the ratio of the number of layers of the mica layer to the resin glass fiber layer is 3:1. The mica layer comprises a mica material and an adhesive in a mass ratio of 100:25, the mica material is a natural mineral material of muscovite mica, and the adhesive is bisphenol A epoxy resin 128 epoxy resin; the resin glass fiber cloth layer comprises a glass fiber cloth and a resin in a mass ratio of 100:65, the glass fiber cloth is an alkali-free glass fiber, and the resin is bisphenol A epoxy resin 128 epoxy resin.

[0049] The preparation method of the mica glass fiber composite material of this embodiment is the same as that of Example 1.

[0050] Example 4

[0051] The mica glass fiber composite material of this embodiment comprises mica layers and resin glass fiber cloth layers connected to each other, with a total number of 16 layers, and the ratio of the number of layers of the mica layer to the resin glass fiber layer is 3:1. The mica layer comprises a mica material and an adhesive in a mass ratio of 100:15, the mica material is a natural mineral material of muscovite mica, and the adhesive is bisphenol A epoxy resin 128 epoxy resin; the resin glass fiber cloth layer comprises a glass fiber cloth and a resin in a mass ratio of 100:65, the glass fiber cloth is an alkali-free glass fiber, and the resin is bisphenol A epoxy resin 128 epoxy resin.

[0052] The preparation method of the mica glass fiber composite material of this embodiment is the same as that of Example 1.

[0053] Example 5

[0054] The mica glass fiber composite material of this embodiment comprises mica layers and resin glass fiber cloth layers connected to each other, with a total number of 16 layers, and the ratio of the number of layers of the mica layer to the resin glass fiber layer is 3:1. The mica layer comprises a mica material and an adhesive in a mass ratio of 100:25, the mica material is a natural mineral material of muscovite mica, and the adhesive is bisphenol A epoxy resin 128 epoxy resin; the resin glass fiber cloth layer comprises a glass fiber cloth and a resin in a mass ratio of 100:45, the glass fiber cloth is an alkali-free glass fiber, and the resin is bisphenol A epoxy resin 128 epoxy resin.

[0055] The preparation method of the mica glass fiber composite material of this embodiment is the same as that of Example 1.

[0056] Example 6

[0057] The mica glass fiber composite material of this embodiment comprises mica layers and resin glass fiber cloth layers connected to each other, with a total number of 16 layers, and the ratio of the number of layers of the mica layer to the resin glass fiber layer is 3:1. The mica layer comprises a mica material and an adhesive in a mass ratio of 100:18, the mica material is a natural mineral material of muscovite mica, and the adhesive is an organic silicone resin SH-5202 methyl silicone resin; the resin glass fiber cloth layer comprises a glass fiber cloth and a resin in a mass ratio of 100:55, the glass fiber cloth is an alkali-free glass fiber, and the resin is an organic silicone resin SH-5202 methyl silicone resin.

[0058] The preparation method of the mica glass fiber composite material of this embodiment is the same as that of Example 1.

[0059] Example 7

[0060] The mica glass fiber composite material of this embodiment comprises mica layers and resin glass fiber cloth layers connected to each other, with a total number of 16 layers, and the ratio of the number of layers of the mica layer to the resin glass fiber layer is 3:1. The mica layer comprises a mica material and an adhesive in a mass ratio of 100:18, the mica material is a natural mineral material of muscovite mica, and the adhesive is 2402 phenolic resin; the resin glass fiber cloth layer comprises a glass fiber cloth and a resin in a mass ratio of 100:55, the glass fiber cloth is an alkali-free glass fiber, and the resin is a silicone resin.

[0061] The preparation method of the mica glass fiber composite material of this embodiment is the same as that of Example 1.

[0062] Example 8

[0063] The mica glass fiber composite material of this embodiment comprises interconnected mica layers and resin glass fiber cloth layers, with a total number of 16 layers, and the ratio of the number of layers of the mica layer to the resin glass fiber layer is 3:1. The mica layer comprises a mica material and an adhesive in a mass ratio of 100:18, and the mica material is a natural mineral material of muscovite mica, and the adhesive is a phenolic resin material produced by Goode Electrical Materials Systems (Suzhou) Co., Ltd.; the resin glass fiber cloth layer comprises a glass fiber cloth and a resin in a mass ratio of 100:55, the glass fiber cloth is an alkali-free glass fiber, and the resin is an epoxy resin.

[0064] The preparation method of the mica glass fiber composite material of this embodiment is the same as that of Example 1.

[0065] Example 9

[0066] The difference between this embodiment and embodiment 1 is that the mica material is replaced by phlogopite instead of muscovite, and the rest is the same as that of embodiment 1.

[0067] Example 10

[0068] The difference between this embodiment and embodiment 1 is that the adhesive is replaced by polyurethane resin instead of epoxy resin, and the rest is the same as that of embodiment 1.

[0069] Embodiment 11

[0070] The difference between this embodiment and embodiment 1 is that the resin is replaced by polyurethane resin instead of epoxy resin, and the rest is the same as that of embodiment 1.

[0071] Comparative Example 1

[0072] The difference between this comparative example and Example 1 is that the mica layer contains mica material and adhesive in a mass ratio of 100:8, and the rest are the same as those in Example 1.

[0073] Comparative Example 2

[0074] The difference between this comparative example and Example 1 is that the mica layer contains mica material and adhesive in a mass ratio of 100:30, and the rest are the same as Example 1.

[0075] Comparative Example 3

[0076] The difference between this comparative example and Example 1 is that the resin glass fiber cloth layer contains glass fiber cloth and resin in a mass ratio of 100:30, and the rest are the same as those in Example 1.

[0077] Comparative Example 4

[0078] The difference between this comparative example and Example 1 is that the resin glass fiber cloth layer contains glass fiber cloth and resin in a mass ratio of 100:80, and the rest are the same as those in Example 1.

[0079] Comparative Example 5

[0080] The mica material of this comparative example is a conventional material in the prior art, and its specific composition is as follows: mica material and adhesive in a mass ratio of 100:15.

[0081] The preparation method is as follows:

[0082] (1) Cut 300*300mm laminated mica paper;

[0083] (2) stacking 16 sheets of mica paper in sequence;

[0084] (3) The stacked mica paper is placed on a hot pressing device, and hot-pressed and cured at 600T pressure and 120°C for 20 minutes to obtain a mica board material.

[0085] The mica glass fiber composite materials prepared in Examples 1-11 and the materials prepared in Comparative Examples 1-5 were subjected to performance tests. The test results are shown in Table 1.

[0086] Among them, the tensile strength test is carried out in accordance with ISO527 standard; the bending strength test is carried out in accordance with ISO178:2010 standard; the impact resistance test is carried out in accordance with ISO179:2010 standard, and the thermal insulation performance test refers to the hot surface 1000±200℃ and measures the cold surface temperature.

[0087] Table 1

[0088]

[0089]

[0090] As can be seen from Table 1, the mica glass fiber composite material of the present invention is thin, light, has good mechanical properties, can withstand high temperatures of 1200°C without deformation, has good thermal insulation, and has strong impact resistance. It can be used for structural parts to protect the bottom of the battery, and can more effectively and comprehensively protect and delay the safety problems caused by thermal runaway of the battery pack. Specifically, the tensile strength of the prepared mica glass fiber composite material is 178-235MPa, the bending strength is 303-350MPa, and the impact resistance is 28.8-36.7KJ / m 2 , the hot surface insulation performance test is 1000±200℃ and the cold surface temperature is 277-295℃.

[0091] In Comparative Example 1, the mass ratio of mica material to adhesive is too large, which will result in insufficient mica content, insufficient product strength and poor thermal insulation effect.

[0092] In Comparative Example 2, the mass ratio of mica material to adhesive is too small, which will result in poor bonding effect and easy delamination of the finished product.

[0093] In Comparative Example 3, the mass ratio of glass fiber cloth to resin is too large, which will result in insufficient glass fiber cloth content and insufficient product strength.

[0094] In Comparative Example 4, the mass ratio of glass fiber cloth to resin is too small, which will result in poor bonding effect and easy delamination of the finished product.

[0095] Comparative Example 5 uses conventional materials, which will reduce the physical strength and thermal insulation effect of the product.

[0096] The present invention illustrates the detailed process equipment and process flow of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed process equipment and process flow, that is, it does not mean that the present invention must rely on the above-mentioned detailed process equipment and process flow to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

[0097] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

[0098] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0099] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. A mica glass fiber composite material, characterized in that: It comprises a mica layer and a resin glass fiber cloth layer connected to each other, wherein the mica layer comprises a mica material and an adhesive in a mass ratio of 100:(10-25), and the resin glass fiber cloth layer comprises a glass fiber cloth and a resin in a mass ratio of 100:(45-65); The mica glass fiber composite material is prepared by the following method: (1) preparing a mica layer material using a mica material and an adhesive as raw materials according to a ratio; (2) preparing a resin glass fiber cloth layer material using glass fiber cloth and resin as raw materials according to a ratio; (3) stacking the mica layer material and the resin glass fiber cloth layer material in a ratio of (2-4):1, and hot pressing and compounding at a temperature of 115-130° C. to obtain the mica glass fiber composite material; The mica glass fiber composite material has a tensile strength of 178-235 MPa, a flexural strength of 303-350 MPa, an impact resistance of 28.8-36.7 KJ / m2, a hot surface 1000±200°C insulation performance test, and a cold surface temperature of 277-295°C.

2. The mica glass fiber composite material according to claim 1, characterized in that: The mica material is phlogopite or muscovite.

3. The mica glass fiber composite material according to claim 1, characterized in that: The adhesive is any one of epoxy resin, silicone resin and phenolic resin or a mixture of at least two of them.

4. The mica glass fiber composite material according to claim 1, characterized in that: The resin is epoxy resin and / or silicone resin.

5. The mica glass fiber composite material according to claim 1, characterized in that: The glass fiber cloth has a thickness of 0.05-0.07 mm and a mesh number of 100-200 meshes.

6. The mica glass fiber composite material according to claim 1, characterized in that: The thickness of the mica layer is 0.2-2 mm, and the thickness of the resin glass fiber cloth layer is 0.05-0.2 mm.

7. A method for preparing a mica glass fiber composite material according to any one of claims 1 to 6, characterized in that: The steps include: (1) preparing a mica layer material using a mica material and an adhesive as raw materials according to a ratio; (2) preparing a resin glass fiber cloth layer material using glass fiber cloth and resin as raw materials according to a ratio; (3) The mica layer material and the resin glass fiber cloth layer material are stacked in a ratio of (2-4):1, and hot-pressed at a temperature of 115-130° C. to obtain the mica glass fiber composite material.

8. The preparation method according to claim 7, characterized in that: The hot pressing pressure is 500-800T.

9. The preparation method according to claim 7, characterized in that: The heat pressing time is 10-30 minutes.

10. An application of the mica glass fiber composite material according to any one of claims 1 to 6, characterized in that: The mica glass fiber composite material is used for preparing structural parts.