A kind of polyhydroxy branched polyetheramine and its preparation method and application

The polyhydroxy branched polyetheramine prepared under catalyst-free conditions solves the complexity of polyetheramine synthesis and the safety of glass cutting fluid additives, provides simplified processes and environmentally friendly lubricating additives, and improves the accuracy and efficiency of glass processing. .

CN115838337BActive Publication Date: 2024-10-25GUANGZHOU TIANRUN NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211476610.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-23
Publication Date
2024-10-25
Estimated Expiration
2042-11-23

AI Technical Summary

Technical Problem

The synthesis reaction conditions of existing branched and hyperbranched polyetheramines are complex and demanding, and the post-reaction treatment steps are cumbersome, which is not conducive to industrialization. At the same time, the additives of existing glass cutting fluids have environmental and safety risks and cannot meet strict environmental and occupational requirements. Health requirements.

Method used

Polyhydroxyl branched polyetheramine was prepared by reacting hydroxyethylethylenediamine and ethylene glycol diglycidyl ether in water under catalyst-free conditions, and was used as a lubricating additive in water-based glass cutting fluid.

Benefits of technology

It realizes the rapid and stable synthesis of polyetheramine, simplifies the process flow, reduces production costs, and provides polyhydroxy branched polyetheramine with good water solubility and good lubricity. As an environmentally friendly glass cutting fluid additive, it improves processing efficiency. Precision and efficiency, extending tool and fluid life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115838337B_ABST
    Figure CN115838337B_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of polyetheramines, and specifically relates to a polyhydroxy branched polyetheramine and a preparation method and application thereof, and provides a polyhydroxy branched polyetheramine which has a simple structure and is convenient for rapid synthesis in industrial production. The polyhydroxy branched polyetheramine can be used as a lubricating additive for water-based cutting fluids used in glass processing, and helps to increase the service life of diamond tools used in glass processing, and has significant substantial characteristics.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyetheramines, and in particular to a polyhydroxy branched polyetheramine and a preparation method and application thereof. Background Art

[0002] Polyetheramines are a class of polymer compounds containing non-polar polyether groups and polar amine structures. They can be divided into three types according to their structures: (1) linear polyetheramines, with a polyether main chain and an amine at the end; (2) branched polyetheramines, with a polyether segment and amine groups alternating in the main chain; and (3) side chain amine polyetheramines, with a polyether main chain and amine groups in the side chain. Polyetheramines with different structures have different synthesis methods and different uses.

[0003] There are many polyetheramines and their synthesis methods. Patent CN106432708A introduces a multi-branched polyetheramine and its preparation method, which are as follows: (1) using propylene glycol, a glycol compound, water and an acidic catalyst to react to obtain an intermediate product; (2) using the intermediate product, a chlorinated epoxide, an alkaline compound and an organic amine to react to obtain a multi-branched polyetheramine. The multi-branched polyetheramine has good shale inhibition, clay hydration dispersibility and good lubricity, and can be used in drilling fluids. It is suitable for highly water-sensitive shale, mudstone-containing and other easily collapsed formations and shale gas horizontal well drilling construction. Patent CN106397766A discloses a method for synthesizing hyperbranched polyetheramine and the method thereof. The specific synthesis method is as follows: 1,8-p-menthanenediamine is dissolved in an organic solvent, and under nitrogen protection, a diepoxy-terminated polyether solution is added dropwise to the reaction solution for reaction. After the reaction is fully reacted, the organic solvent is removed by vacuum distillation, and the white paste obtained by solvent sedimentation is vacuum dried to obtain a hyperbranched polyetheramine, which is further modified to obtain a hyperbranched polyetheramine hydrogel.

[0004] The synthesis of branched and hyperbranched polyetheramines involved in the above patents requires the use of catalysts for multi-step reactions; or the use of organic solvents, which are removed by distillation after the reaction. The reaction conditions are complex and demanding, and the post-reaction treatment steps are cumbersome, which increases equipment and production costs and is not conducive to industrialization.

[0005] On the other hand, water-soluble polyetheramines are expected to be used as lubricating additives for glass cutting fluids.

[0006] Specifically, glass is a hard and brittle non-metallic material, and cutting and grinding of glass products are usually performed using tools and grinding heads with diamonds on the surface. During the processing, a large amount of glass powder and heat will be formed in the processing area, which will have an adverse effect on the processing accuracy and efficiency, so it is necessary to absorb the heat and take away the glass powder by spraying glass cutting fluid. However, glass powder is often fine in particles and is not easy to settle in the cutting fluid. If the sedimentation is not timely, the glass powder will be recirculated to the processing area with the cutting fluid and cause secondary damage to the glass to be processed, which is a huge damage to the mobile phone touch screen glass and optical lens glass. It can be seen that the cutting fluid used in the processing of such glass must have good sedimentation, low foaming and lubricity, and from the perspective of the protection of machine tools and metal parts, the glass cutting fluid also needs certain anti-rust properties. Under the processing conditions of high speed and high feed rate, the processing accuracy, efficiency and yield of the common glass cutting fluid on the market cannot meet the processing requirements of the above-mentioned glass at the same time.

[0007] And along with the gradual strengthening of enterprise environmental awareness and occupational health risk prevention awareness, the safety and environmental protection requirements of glass cutting fluid are more stringent.Existing glass cutting fluid mostly uses quaternary ammonium salt cationic additives to improve sedimentation performance, such as the patented products of application publication number CN102102008A and CN103275803 A, but most quaternary ammonium salts all contain halogen ions such as chloride ions or bromide ions, which cannot be applied to the occasions requiring halogen-free.In addition, quaternary ammonium salt cationic additives are adsorbed on the surface of electronegative organism cells under the action of electrostatic force, destroy cell membrane, denature protein, present bactericidal properties, and also just based on the same mechanism of action, it has larger irritation to human skin and mucous membrane, due to the general barehanded operation of the operator, direct contact with workpiece and cutting fluid, therefore the glass cutting fluid adding quaternary ammonium salt cationic additives cannot meet the requirements of environmental protection and occupational safety and health.More traditional glass cutting fluids use suspected carcinogen nitrite, which has aggravated the harm to the health of the operator. Some additives in cutting fluids can also cause harm to the environment. For example, the patent with authorization announcement number CN103275803 A uses the phosphorus-containing raw material inositol hexaphosphate as a cleaning agent. This additive can easily cause eutrophication of water bodies, which is not conducive to the management and protection of the water environment.

[0008] Therefore, in the patent document with the patent number CN106675751A and the name "Glass Cutting Fluid", a glass cutting fluid is disclosed, which includes the components of: polyol, water-soluble lubricant, carboxylate rust inhibitor, sedimentation agent and defoamer. In addition, in the description of the patent document, paragraph

[0034] , it is mentioned that "the water-soluble lubricant is selected from at least one of polyethylene glycol with a number average molecular weight of 200 to 2000, glycerol polyoxyethylene ether with a number average molecular weight of 500 to 3000, or water-soluble polyether. The water-soluble lubricant can make the lubricant fully dissolve in the water solvent, and ensure that the glass cutting fluid has good lubrication performance, avoiding damage to the glass by the tool during the glass cutting process and damage to the glass by glass chips and glass powder." And water-soluble polyether amine is one of the water-soluble polyethers.

[0009] In summary, the development of a new water-soluble polyetheramine with simple synthesis process and simple post-treatment has important research significance and application value. Summary of the invention

[0010] In order to solve the problems that the synthesis reaction conditions of existing branched and hyperbranched polyetheramines are complex and demanding, the post-reaction treatment steps are cumbersome and not conducive to industrialization, so as to quickly and stably prepare water-soluble polyetheramines, a polyhydroxy branched polyetheramine and a preparation method thereof are provided.

[0011] Another object of the present invention is to provide the use of the above-mentioned polyhydroxy branched polyether amine in water-based cutting fluid for glass processing.

[0012] The first aspect of the present invention provides a polyhydroxy branched polyetheramine, the structural formula of which is:

[0013]

[0014] Wherein, n is an integer of 5-30.

[0015] Preferably, n is an integer of 10-20.

[0016] The second aspect of the present invention provides a method for preparing the above-mentioned polyhydroxy branched polyetheramine, comprising the following steps:

[0017] Add water to the reflux reaction vessel;

[0018] Add hydroxyethylethylenediamine to a reflux reaction vessel and mix with water;

[0019] Slowly add ethylene glycol diglycidyl ether dropwise to the mixture of hydroxyethylethylenediamine and water;

[0020] The reaction conditions are maintained to obtain a polyhydroxy branched polyetheramine aqueous solution.

[0021] Furthermore, the molar ratio of the hydroxyethylethylenediamine to ethylene glycol diglycidyl ether is 1 to 3:1.

[0022] Furthermore, the mass fraction of the water is 30-50%.

[0023] Furthermore, the reaction temperature is 70-100° C., and the reaction time is 2-4 hours.

[0024] Furthermore, the method also includes drying the prepared polyhydroxy branched polyetheramine aqueous solution to remove water.

[0025] The third aspect of the present invention provides the use of the above-mentioned polyhydroxy branched polyetheramine as a lubricating additive in the preparation of a water-based cutting fluid for glass processing.

[0026] The advantages of the present invention are:

[0027] The polyhydroxy branched polyetheramine provided by the present invention has good water solubility and lubricity, and can be used as a lubricant; and can be synthesized using water as a solvent under catalyst-free conditions, and the operation and reaction conditions are simple; and because no organic solvent is required, cumbersome post-processing steps are avoided, which is conducive to industrial promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0029] Figure 1 is the infrared spectrum of the polyhydroxy branched polyetheramine of Example 1;

[0030] Figure 2 is the infrared spectrum of the polyhydroxy branched polyetheramine of Example 2;

[0031] Figure 3 This is the infrared spectrum of the polyhydroxy branched polyetheramine of Example 3. DETAILED DESCRIPTION

[0032] In order to solve the problems that the synthesis reaction conditions of existing branched and hyperbranched polyetheramines are complex and demanding, the post-reaction treatment steps are cumbersome and not conducive to industrialization, so as to quickly and stably prepare polyetheramines and then effectively apply polyetheramines to cutting fluid lubricants, a polyhydroxy branched polyetheramine and a preparation method and application thereof are provided.

[0033] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] It should be noted that the terms such as "within", "in" and "a" etc. cited in this specification are only for the convenience of description and are not used to limit the scope of the present invention. Changes or adjustments in their relative relationships, without substantially changing the technical content, should also be regarded as the scope of the present invention, and it is necessary to make it clear in advance.

[0035] In the description of the present invention, it should be understood that the terms "upper", "lower", "front", "rear", "left", "right", "vertical", "horizontal", etc. indicate the orientation or position relationship based on the orientation or position relationship shown in the drawings, which is only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", etc. are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first", "second", etc. may explicitly or implicitly include one or more of the features. In the description of the present invention, it should be noted that, unless otherwise clearly specified and defined, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be directly connected, or indirectly connected through an intermediate medium, or it can be the internal communication of two elements. For those of ordinary skill in the art, the specific meanings of the above terms in the present invention can be understood by specific circumstances.

[0036] The structural formula of the polyhydroxy branched polyetheramine provided in each embodiment of the present invention is as follows:

[0037]

[0038] Wherein, n is an integer of 5-30.

[0039] Preferably, n is an integer of 10-20.

[0040] Example 1

[0041] This embodiment provides a polyhydroxy branched polyetheramine, which is prepared by the following process:

[0042] Weigh 312g (3mol) of hydroxyethylethylenediamine and add it to a four-necked reaction flask (reflux reaction vessel) equipped with a stirrer, a thermometer, a reflux condenser and a dropping funnel, add 834g of water, and slowly drop 522g (3mol) of ethylene glycol diglycidyl ether. During the dropwise addition, the reaction temperature is controlled at 80-90°C. After the dropwise addition is completed, the reaction temperature is continued to be maintained at 80-90°C, and the reaction is carried out for 3.5 hours to obtain a light yellow transparent polyetheramine aqueous solution. The viscosity is measured by a NDJ-7 rotary viscometer to be 78mPa·s (25°C). After drying and removing water, a polyhydroxy branched polyetheramine is obtained.

[0043] The above polyhydroxy branched polyetheramine was subjected to infrared spectroscopy analysis. Figure 1 The infrared spectrum of the obtained polyhydroxy branched polyetheramine was measured by KBr smear method. From the spectrum, we can see that: 3373.78cm-1 is the stretching vibration absorption peak of hydroxyl group, 2914.44cm-1 and 2871.74cm-1 are the stretching vibration absorption peaks of CH, 1456.51cm-1 and 1355.15cm-1 are the CH2 variable angle vibration absorption peaks, and the broad peak at 1111.90cm-1 is the mixed peak of COC and CO stretching vibration absorption peaks in COH.

[0044] Example 2

[0045] This embodiment provides a polyhydroxy branched polyetheramine, which is prepared by the following process:

[0046] Weigh 416g (4mol) of hydroxyethylethylenediamine and add it to a four-necked reaction flask equipped with a stirrer, a thermometer, a reflux condenser and a dropping funnel, add 510g of water, and slowly drop 348g (2mol) of ethylene glycol diglycidyl ether. During the dropwise addition, the reaction temperature is controlled at 85-90°C. After the dropwise addition is completed, the reaction temperature is continued to be maintained at 85-95°C, and the reaction is carried out for 3 hours to obtain a light yellow transparent polyetheramine aqueous solution. The viscosity is measured by a NDJ-7 rotary viscometer to be 120mPa·s (25°C), and the polyhydroxy branched polyetheramine is obtained after drying and dehydration.

[0047] The above polyhydroxy branched polyetheramine was subjected to infrared spectrum analysis. Figure 2 This is the infrared spectrum of the obtained polyetheramine, 3373.68cm-1 is the stretching vibration absorption peak of hydroxyl, 2924.40cm-1 and 2872.02cm-1 are the stretching vibration absorption peaks of CH, 1457.08cm-1 and 1354.98cm-1 are the CH2 angle vibration absorption peaks, and the peaks at 1115.64cm-1 and 1061.76cm-1 are the mixed peaks of the stretching vibration absorption peaks of COC and COH.

[0048] Example 3

[0049] This embodiment provides a polyhydroxy branched polyetheramine, which is prepared by the following process:

[0050] Weigh 624g (6mol) of hydroxyethylethylenediamine and add it to a four-necked reaction flask equipped with a stirrer, a thermometer, a reflux condenser and a dropping funnel, add 416g of water, and slowly drop 348g (2mol) of ethylene glycol diglycidyl ether. During the addition process, control the reaction temperature at 90-95°C. After the dropwise addition is completed, continue to maintain the reaction temperature at 90-95°C, react for 2.5 hours, and obtain a light yellow transparent polyetheramine aqueous solution. The viscosity is 430mPa·s (25°C) measured by a NDJ-7 rotary viscometer. After drying and removing water, obtain a polyhydroxy branched polyetheramine.

[0051] The above polyhydroxy branched polyetheramine was subjected to infrared spectrum analysis. Figure 3 This is the infrared spectrum of the obtained polyetheramine, 3362.39 cm-1 is the stretching vibration absorption peak of hydroxyl, 2926.79 cm-1 and 2867.26 cm-1 are the stretching vibration absorption peaks of CH, 1470.60 cm-1 and 1354.70 cm-1 are the CH2 variable angle vibration absorption peaks, and the peaks at 1117.50 cm-1 and 1060.62 cm-1 are the mixed peaks of the stretching vibration absorption peaks of COC and COH.

[0052] The polyhydroxy branched polyetheramine provided in Examples 1 to 3 was prepared into a 50% by mass aqueous solution, and its maximum no-seizure load PB value was measured according to GB / T 3142-1982 (2004). The results are shown in Table 1.

[0053] Table 1 Performance test results of polyhydroxy branched polyetheramine aqueous solutions provided in Examples 1 to 3

[0054]

[0055] As shown in Table 1, the polyhydroxy branched polyetheramine provided by each embodiment of the present invention has good water solubility, and the maximum no-seizure load PB value of its 50% aqueous solution is ≥850N (GB / T 3142-1982 (2004)), has lubricity, and can be used as a lubricating additive.

[0056] The following examples provide a series of water-based cutting fluids for flat glass processing, and the preparation process is as follows:

[0057] Example 4

[0058] 5000g of water-based cutting fluid was prepared. In this embodiment 4, the polyhydroxy branched polyetheramine synthesized in embodiment 1 was used as a lubricating additive, triethanolamine was selected as a chemical self-sharpening agent, and auxiliary agents such as anti-wear agent, buffer, defoamer and bactericide were added. The rest was tap water. The water-based cutting fluid for flat glass processing was prepared. The mass fractions of each component were:

[0059]

[0060]

[0061] Under stirring conditions, add triethanolamine, polyetheramine, anti-wear agent, buffer, defoamer and bactericide to weighed tap water in proportion, stir evenly to get 5000g water-based cutting fluid. When using, use it in a dilution ratio of 1:15 (cutting fluid: water) with diamond tools for flat glass drilling, edge grinding, chamfering, cutting and other processing processes.

[0062] Example 5

[0063] 5000g of water-based cutting fluid was prepared. In this embodiment 5, the polyhydroxy branched polyetheramine synthesized in embodiment 2 was used as a lubricating additive, triethanolamine was selected as a chemical self-sharpening agent, and auxiliary agents such as anti-wear agents, buffers, defoamers and bactericides were added. The rest was tap water. The water-based cutting fluid for flat glass processing was prepared. The mass fractions of the components were:

[0064]

[0065] Under stirring conditions, add triethanolamine, polyetheramine, anti-wear agent, buffer, defoamer and bactericide to weighed tap water in proportion, stir evenly to get 5000g water-based cutting fluid. When using, use it in a dilution ratio of 1:15 (cutting fluid: water) with diamond tools for flat glass drilling, edge grinding, chamfering, cutting and other processing processes.

[0066] Example 6

[0067] 5000g of water-based cutting fluid was prepared. In this embodiment 6, the polyhydroxy branched polyetheramine synthesized in embodiment 3 was used as a lubricating additive, triethanolamine was selected as a chemical self-sharpening agent, and auxiliary agents such as anti-wear agents, buffers, defoamers and bactericides were added. The rest was tap water. The water-based cutting fluid for flat glass processing was prepared. The mass fractions of each component were:

[0068]

[0069]

[0070] Under stirring conditions, add triethanolamine, polyetheramine, anti-wear agent, buffer, defoamer and bactericide to weighed tap water in proportion, stir evenly to get 5000g water-based cutting fluid. When using, use it in a dilution ratio of 1:15 (cutting fluid: water) with diamond tools for flat glass drilling, edge grinding, chamfering, cutting and other processing processes.

[0071] The water-based cutting fluid of the present invention and the domestic water-based cutting fluid used in a flat glass processing plant for the same processing technology (referred to as comparative example 1) were compared under the same processing parameter conditions to compare the technical indicators such as the qualified rate of the processed workpieces, the service life of the diamond tools and the cutting fluid. The specific results are shown in Table 2:

[0072] Table 2 Comparison of the application effects of the cutting fluids of each embodiment with other cutting fluids

[0073]

[0074] It can be seen from Table 2 that the cutting fluid provided by each embodiment of the present invention can meet the processing requirements of flat glass drilling, edging, chamfering, cutting, etc., extend the service life of diamond tools, and extend the service life of cutting fluid.

[0075] The polyhydroxy branched polyetheramine synthesized by using hydroxyethylethylenediamine and ethylene glycol diglycidyl ether in a molar ratio of 3:1 in Example 3 has the largest no-seizure load PB value of 50% aqueous solution, and the service life of diamond tools is the longest when used as a lubricating additive for water-based cutting fluid. Therefore, it can be considered that the amount of hydroxyethylethylenediamine used within a certain range is positively correlated with the lubricating performance of the polyhydroxy branched polyetheramine obtained.

[0076] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit the protection scope of the present invention. For ordinary technicians in this field, other different forms of changes or modifications can be made based on the above descriptions and ideas. It is not necessary and impossible to list all the implementation methods here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. An application of a polyhydroxy branched polyetheramine, characterized in that: The polyhydroxy branched polyetheramine is used as a lubricating additive in the preparation of a water-based cutting fluid for glass processing. The structural formula of the polyhydroxy branched polyetheramine is: Wherein, n is an integer of 5-30.

2. The use of a polyhydroxy branched polyetheramine according to claim 1, characterized in that: The preparation method of the polyhydroxy branched polyetheramine comprises the following steps: Add water to the reflux reaction vessel; Add hydroxyethylethylenediamine to a reflux reaction vessel and mix with water; Slowly add ethylene glycol diglycidyl ether dropwise to the mixture of hydroxyethylethylenediamine and water; The reaction conditions are maintained to obtain a polyhydroxy branched polyetheramine aqueous solution.

3. The use of a polyhydroxy branched polyetheramine according to claim 2, characterized in that: The molar ratio of the hydroxyethylethylenediamine to ethylene glycol diglycidyl ether is 1 to 3:

1.

4. The use of a polyhydroxy branched polyetheramine according to claim 2, characterized in that: The mass fraction of the water is 30-50%.

5. The use of a polyhydroxy branched polyetheramine according to claim 2, wherein the reaction temperature is 70-100°C and the reaction time is 2-4 hours.