A method for preparing a hydrorefining catalyst

Through the use of potassium hydroxide spraying and polyamine complexing agent, the problems of poor dispersion and high cost of active components in the hydrorefining catalyst are solved, the hydrogenation performance and stability of the catalyst are improved, and the preparation process is simplified.

CN115845866BActive Publication Date: 2024-11-26PETROCHINA CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111112360.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-09-23
Publication Date
2024-11-26
Estimated Expiration
2041-09-23

AI Technical Summary

Technical Problem

In the existing preparation methods for hydrogenation purification catalysts, it is difficult to form efficient dispersion of active components on the support, resulting in low catalyst activity and high cost, and difficult to control the calcination temperature, which easily produces fly temperature and gas emission, resulting in large losses.

Method used

The carrier is pre-sprayed with potassium hydroxide solution to release adsorption heat, reduce the acidity of the carrier surface, and form a stable complex with the active components through a polyamine complexing agent, thereby improving the dispersion of the active components and the hydrogenation of the catalyst. performance.

Benefits of technology

The hydrogenation performance and stability of the catalyst are improved, the life of the catalyst is extended, the active components are highly dispersed on the support, the gas discharge and loss during the calcination process is reduced, and the preparation process is simplified.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003274327950000161
    Figure BDA0003274327950000161
  • Figure BDA0003274327950000162
    Figure BDA0003274327950000162
  • Figure BDA0003274327950000171
    Figure BDA0003274327950000171
Patent Text Reader

Abstract

The present invention relates to a preparation method of a hydrorefining catalyst, wherein the carrier of the catalyst is a high temperature resistant inorganic oxide, the catalyst contains potassium, a part of the potassium is introduced by pre-spraying the carrier; a part of the potassium is introduced by impregnating the carrier with an active component impregnation solution containing potassium, and the carrier needs to be aged after spraying before being impregnated with the active component solution. When the catalyst prepared by the method of the present invention is used for hydrodesulfurization, it can hydrogenate saturated monoolefins to the maximum extent, and is particularly suitable for oil products with variable sulfur content and diene content, and can also meet the requirements of high space velocity operation, and the catalyst has excellent hydrodesulfurization performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a catalyst, in particular to a method for preparing a hydrogenation refining catalyst. Background Art

[0002] Hydrofining technology is the main means to improve the quality of petrochemical products, and its core is hydrofining catalysts. Hydrofining catalysts are divided into supported and unsupported types. Supported catalysts are mainly used in industry today. Supported hydrofining catalysts are generally made by impregnating active metals (Mo, W, Ni, Co, etc.) onto a carrier. The active components of the catalyst prepared by the impregnation method are distributed on the inner and outer surfaces of the catalyst carrier, including the inner surfaces of deep internal voids and pores. There are many reports on the preparation methods of hydrofining catalysts, which mainly focus on preparation methods and process research, carrier modification, and additive addition.

[0003] Introducing additives into catalysts is one of the most common means to improve the activity of hydrogenation catalysts. Common additives for hydrorefining catalysts include first additives such as cobalt and nickel and second additives such as phosphorus and boron. At the same time, the application of chelating agents and other active component solutions as complexing components such as citric acid, phosphoric acid, ethylenediamine, ethylenediaminetetraacetic acid, ethylene glycol, etc. in the preparation of hydrorefining catalysts has achieved good results.

[0004] ZL201510700293.9 relates to a hydrogenation catalyst and a preparation method thereof, the preparation method comprising: (1) using an impregnation method to load a water-soluble salt of a hydrogenation metal active component and an organic complexing agent onto a carrier, and then drying and roasting to obtain a semi-finished catalyst, wherein the roasting conditions are such that the carbon content in the semi-finished catalyst is 0.03-0.5% by weight based on the total amount of the semi-finished catalyst; (2) using a solution containing an organic complexing agent as an impregnation liquid to impregnate the semi-finished catalyst obtained in step (1), and then drying without roasting; (3) loading a metal element as an auxiliary agent onto the carrier; wherein step (3) is performed at any one or more of before, during and after step (1) and before step (2). This patent adopts a three-step impregnation method to prepare the catalyst, which consumes a lot of manpower and material resources, and will cause a significant increase in the cost of catalyst preparation.

[0005] ZL91110935.8 discloses a method for preparing a cobalt-molybdenum hydrorefining catalyst, wherein cobalt acetate is dissolved in water and then ethylenediamine is added, wherein the molar ratio of cobalt acetate to ethylenediamine is 1:1.5-3, so as to form a mixed solution of cobalt-ethylenediamine, and concentrated ammonia is added to the solution to adjust the pH value to 12-14, and then ammonium molybdate is added to fully dissolve the solution to prepare a co-impregnation solution containing cobalt-molybdenum metals, and a porous carrier is impregnated with the solution to prepare a catalyst. The disadvantage of this method is that the catalyst product needs to be calcined in an oxygen-free or micro-oxygen atmosphere.

[0006] US4409131 discloses a method for preparing a CoMo / NiMo catalyst, which is prepared by impregnating a carrier with a solution containing an active component and ammonia water in one step. The method describes in detail the preparation process of the active component impregnation solution. During the preparation of the impregnation solution, the mixture needs to be heated to promote the dissolution of the active component.

[0007] US6013598 discloses a method for preparing a selective hydrodesulfurization catalyst, which is composed of active components cobalt, molybdenum and carrier aluminum oxide. The catalyst is prepared by impregnating the carrier with an equal volume of an aqueous solution containing the active components and added with citric acid. The catalyst obtained by this method has a maximum molybdenum oxide content of only 10wt%.

[0008] ZL00130284.1 relates to a second-stage hydrorefining catalyst for cracked gasoline and a preparation method thereof, wherein alumina precursor is used, and when it is formed, a polymer and a metal of the Group IV are added, and the carrier containing the metal of the Group IV is obtained after drying and roasting, and then impregnated with an ammonia co-impregnation solution containing active components of molybdenum, cobalt and nickel, and then dried and roasted to obtain a catalyst. The addition of the metal of the Group IV adjusts the acidity and alkalinity of the carrier and inhibits the coking and deactivation rate of the catalyst.

[0009] ZL99113281.5 relates to a distillate oil hydrorefining catalyst and a preparation method thereof. The catalyst uses alumina or silicon-containing alumina as a carrier, adds a phosphorus additive, and uses W, Mo, and Ni as active components. The staged co-impregnation technology is used to impregnate the prepared W, Mo, Ni, and P co-impregnation solution multiple times to finally prepare the catalyst.

[0010] ZL00122922.2 discloses a distillate oil hydrodesulfurization catalyst and preparation method, wherein the catalyst uses alumina or silicon-containing alumina as a carrier, Mo-Ni as an active component, and a phosphorus additive. The carrier is impregnated in stages using an alkaline Mo-Ni-P co-impregnation solution, and then the co-impregnation is performed in a step-by-step co-impregnation manner. The catalyst is prepared in two or more steps.

[0011] The document "Development of Co-Mo-Ni-W / γ-Al2O3 Diesel Hydrogenation Refining Catalyst" investigated the effects of pore-enlarging agent and calcination temperature on the physical and chemical properties of the carrier and the effects of the preparation method of the impregnation solution on its stability. There are two main methods for preparing the impregnation solution disclosed: (1) low-temperature method: ① heat deionized water and phosphoric acid, add basic nickel carbonate (or basic cobalt carbonate) and molybdenum trioxide, continue heating and stirring until dissolved, cool to room temperature for use; ② add ammonium metatungstate and cobalt acetate (or nickel nitrate) to slightly hot deionized water, stir to dissolve, cool to room temperature for use; ③ mix the cooled ammonium metatungstate and cobalt acetate (or nickel nitrate) solution with the nickel (cobalt) molybdenum phosphorus solution prepared in ①, stir evenly and set to volume for use. (2) High temperature method: dissolve molybdenum trioxide, phosphoric acid and basic nickel carbonate (or basic cobalt carbonate) in deionized water, heat and stir until completely dissolved, then add ammonium metatungstate and cobalt acetate (or nickel nitrate), continue heating and stirring until completely dissolved into a clear solution, then set to volume for use. In the process of preparing the impregnation solution, heating and adding inorganic acid are required.

[0012] CN110465304A discloses a method for preparing a high-activity hydrodesulfurization catalyst, which is to use a carbon-based material as a carrier, perform surface modification on the carbon-based material, prepare a hydrodesulfurization precursor solution containing Ni, Mo, Co, Mo, or Ni, Mo active components, immerse the modified carbon-based material in the precursor solution, immerse the active components on the carrier surface, and obtain a carbon-based hydrodesulfurization catalyst containing NiMo, CoMo, or NiMo active components. The present invention can enrich the surface of the carbon carrier with hydroxyl groups by performing surface treatment on the carbon material carrier, such as oxidation with an oxidizing acid or treatment with an oxidizing gas. By adjusting the degree of treatment, the active components can be changed from a single-layer dispersion to a few layers and multiple layers on the carrier.

[0013] CN94114194.2 discloses a hydrocarbon hydrodesulfurization catalyst and preparation method, wherein the catalyst is prepared by one-time impregnation of cobalt and molybdenum co-impregnation solution using zinc oxide modified γ-Al2O3 as carrier, cobalt and molybdenum as active components. The prepared catalyst has the following composition: CoO 1-10wt%, MoO3 5-18wt%, ZnO 1-15wt%, and the balance is γ-Al2O3. However, the long-term stability of the catalyst operation effect needs further investigation.

[0014] The active components of supported catalysts (especially under conditions of high active component content) are difficult to form a monolayer dispersion or reach the dispersion threshold on the surface of the carrier. The appropriate degree of interaction between the active components and the carrier is one of the main factors affecting the effective loading of the catalyst. Generally speaking, the higher the dispersion of the active components on the carrier, the more effective active sites there are, and the higher the activity of the catalyst. However, the long-term stability of the catalyst must also be considered comprehensively. Therefore, how to improve the interaction between the active components and the carrier to increase the effective loading of the active components on the carrier is the focus of the research and development of hydrotreating catalysts.

[0015] The prepared active component impregnation solution is directly related to the dispersion of the active components in the catalyst after impregnation, thus affecting the performance of the catalyst. The selection of effective solvents and dissolution methods is the key to preparing the impregnation solution. In the process of preparing catalysts containing components such as molybdenum and cobalt by impregnation, the main problem is that the active components Co, Mo, etc. are difficult to dissolve, especially when two or more active components are dissolved in one solvent at the same time. The preparation of catalysts by step-by-step impregnation will increase the cost of catalyst preparation. The problem with the prior art of preparing catalysts by one-step impregnation is that it is necessary to add organic acid / base to promote the dissolution of active components. When a higher content of active components is required, a large amount of organic acid / base needs to be used. The temperature is difficult to control during roasting, and it is easy to produce a temperature runaway phenomenon. In addition, a large amount of gas will be released, and the catalyst loss is also large.

[0016] At present, it is a well-known technology to use ammonia water as a solvent to dissolve active components such as Co, Mo, W, and Ni, but the effect of ammonia water on improving the dispersion of active components is not obvious. In the research on preparation methods and processes, how to simply prepare an impregnation solution containing active components and achieve the requirements of multi-component one-step impregnation without heating, and keep the active components highly dispersed after impregnation, is still a difficult problem. Summary of the invention

[0017] The purpose of the present invention is to provide a method for preparing a hydrorefining catalyst, wherein the prepared catalyst has the characteristics of reasonable distribution of active components and excellent hydrogenation performance.

[0018] A method for preparing a hydrorefining catalyst, wherein the catalyst carrier is a high temperature resistant inorganic oxide, the catalyst contains potassium, a portion of the potassium is added by pre-spraying the carrier, and a portion of the potassium is introduced by impregnating the carrier with an active component impregnation solution containing potassium. After spraying, the carrier needs to be aged before being impregnated with the active component solution.

[0019] The inventors have found that the active component impregnation step in the prior art contains a process of concentrated release of adsorption heat, which affects the dispersion state of the active components and the physicochemical properties of the catalyst in the later stage.

[0020] The invention provides a method for preparing a supported catalyst, wherein a catalyst carrier is subjected to an atomized spray treatment of a potassium hydroxide solution, thereby pre-releasing part of the adsorption heat in the catalyst preparation process, and at the same time, alkali metal potassium can interact with the carrier to reduce the surface acidity of the carrier.

[0021] The catalyst carrier of the present invention is not particularly limited. The carrier used for common supported hydrorefining catalysts is, for example, a high temperature resistant inorganic oxide such as one or more of alumina, silicon oxide, titanium oxide, and zirconium oxide. The carrier is preferably an alumina carrier.

[0022] The water absorption rate of the carrier of the present invention is 80% to 120%, preferably 85% to 110%, and the water absorption rate is hereinafter represented as X (such as the water absorption rate is 90%, X=0.9), and the mass of the sprayed carrier is represented as T grams.

[0023] The spraying step described in the present invention is before the active component is loaded.

[0024] The spraying process uses conventional spray equipment, and the spraying completion time is 1 min to 20 min, preferably 3 min to 10 min.

[0025] The amount of potassium hydroxide solution in the catalyst carrier atomization spraying process is 1%X×T ml to 20%X×T ml, preferably 5%X×T ml to 10%X×T ml. The percentage (volume percentage) of potassium hydroxide solution added is 1% to 20% of the total impregnation solution volume (including the potassium hydroxide solution volume and the active component impregnation solution volume), preferably 5% to 10%.

[0026] After spraying, the carrier needs to be aged for a certain period of time, and the catalyst preparation is directly carried out without drying and calcination. The aging time is 5min to 30min, preferably 10min to 20min.

[0027] The carrier is pre-sprayed with potassium hydroxide solution, the concentration of which is 0.1% to 5%, preferably 0.5% to 1%. The preparation method is: potassium hydroxide is dissolved in deionized water, and the pH value of the prepared potassium hydroxide solution is 12.2 to 13.5.

[0028] The method of the present invention does not limit the specific composition of the catalyst, and the composition of the active components of the catalyst can be adjusted as needed. Due to the use of the method of the present invention, the prepared catalyst exhibits a more excellent hydrorefining effect.

[0029] The present invention also provides a method for preparing an active component impregnation solution containing potassium, wherein potassium hydroxide, ammonia water, a polyamine complexing agent and deionized water are mixed to prepare a composite solvent, and a salt containing the active component is added to the composite solvent to prepare a catalyst by one-step impregnation.

[0030] The present invention does not impose any particular limitation on the concentration of ammonia water used to prepare the active component impregnation solution, and the conventional selection in the art can be adopted. According to the amount of active component added, each active component can be completely dissolved, and at this time, the active component and the polyamine complexing agent form a relatively stable complex.

[0031] The impregnation liquid used in the present invention is an alkaline impregnation liquid, and after the active component is dissolved, the pH value of the impregnation liquid needs to be adjusted to above 10, preferably 10 to 12. The prepared impregnation liquid is clear, stable, and has low surface tension and viscosity.

[0032] The volume of the active component impregnation solution is 1.05×(1-the percentage of potassium hydroxide solution added)X×Tml to 1.25×(1-the percentage of potassium hydroxide solution added)X×T ml, and the preferred volume is 1.10×(1-the percentage of potassium hydroxide solution added)X×T ml to 1.20×(1-the percentage of potassium hydroxide solution added)X×T ml.

[0033] The active component impregnation liquid can be prepared at room temperature (generally defined as 10°C to 30°C, preferably 15°C to 25°C) without the need for a heating process. The present invention is particularly suitable for the preparation of catalysts with multiple active components and high active component content, especially a catalyst preparation method in which the active components are loaded onto a carrier by one-step impregnation, the active components are highly dispersed on the catalyst, and the B acid center on the catalyst is effectively eliminated, and the strong L acid center is weakened.

[0034] The solvent used to dissolve the active components of the present invention is ammonia water added with a polyamine complexing agent and potassium hydroxide. The composite solvent improves the solubility of the active components in ammonia water and reduces the amount of ammonia water used. On the other hand, the addition of the polyamine complexing agent significantly improves the dispersion of the active components of the catalyst. Potassium hydroxide enhances the alkalinity of the impregnation solution, thereby allowing the metal active components to be better complexed with the polyamine complexing agent, improving the stability of the impregnation solution, and also plays a role in adjusting the acidity of the catalyst and improving the hydrogenation refining performance of the catalyst.

[0035] The active components of the catalyst are not specifically limited and are determined according to the purpose of hydrogenation, etc. After the active components are loaded, they need to be aged, dried and calcined. Before impregnating the active components, a certain concentration of potassium hydroxide solution is used to spray the catalyst carrier to release heat and at the same time play a role in carrier modification.

[0036] In the preparation method of the hydrotreating catalyst described in the present invention, the active component is preferably one or more of molybdenum, tungsten, cobalt and nickel, the molybdenum is calculated as molybdenum trioxide, the tungsten is calculated as tungsten trioxide, the cobalt is calculated as cobalt oxide, the nickel is calculated as nickel oxide, and the mass fraction of the active component is greater than or equal to 20% based on the total mass of the carrier as 100%.

[0037] In the present invention, the active component molybdenum is preferably added in the form of ammonium molybdate, and tungsten can be added in the form of ammonium metatungstate, tungstic acid or other alkaline tungstates, preferably ammonium metatungstate. The active components cobalt and nickel can be added in the form of sulfates, halides, nitrates or acetates, preferably nitrates and / or acetates, because nitrates and acetates have good solubility, which is conducive to the distribution of the active components on the carrier.

[0038] The polyamine complexing agent of the present invention is a C2-C7 compound containing one or more NH groups, which can be ethylenediaminetetraacetic acid, a primary amine, a secondary amine or a tertiary amine, preferably ethylenediamine.

[0039] The amount of polyamine complexing agent added varies according to the amount of active components added, and the present invention does not particularly limit it. It is preferably 3 to 9% (volume content) of the amount of the impregnation solution. Too high an amount may easily cause a large amount of organic matter to decompose during the roasting process, while too low an amount may not achieve the effect of promoting the dissolution of active components and improving the dispersion of active components.

[0040] After spraying and impregnation of active component solution by the method of the present invention, the catalyst is obtained by aging, drying and activation. Aging, drying and activation are all completed by existing technologies, and the present invention has no special requirements. The conditions and methods of aging, drying and roasting can refer to the existing technology. It is recommended to dry at 80-120°C for 2-6 hours and roast at 350-600°C for 3-8 hours.

[0041] The potassium oxide content in the finally prepared catalyst is 0.3% to 5%, preferably 0.5% to 2.5%.

[0042] The inventors have found through experimental research that the supported catalyst carrier will release a large amount of adsorption heat in the process of impregnation with the active component impregnation solution, which affects the dispersion state of the active component and the physicochemical properties of the catalyst in the later stage. By pre-spraying potassium hydroxide solution and then impregnating the active component impregnation solution, not only can the hydrogenation performance of the catalyst be improved, but also the life of the catalyst can be effectively extended. It is speculated that the reason may be that: the pre-sprayed potassium hydroxide solution, on the one hand, releases part of the adsorption heat of the carrier in advance, so that part of the adsorption heat of the catalyst carrier in the process of impregnating the active component is released in advance; on the other hand, the pre-sprayed potassium hydroxide solution changes the number and arrangement of hydroxyl groups on the surface of the catalyst carrier, which improves the dispersibility of the active component in the subsequent impregnation process of the active component. At the same time, the pre-sprayed solution occupies relatively deep holes in advance due to the capillary effect, so that the active components of the catalyst form a gradient distribution, and the active components are dispersed more efficiently and more evenly.

[0043] The present invention discloses a hydrorefining catalyst and a preparation method thereof, which overcomes the impregnation effect and active component clustering effect brought about by conventional impregnation methods, improves the loading effect of active metal components, forms a certain gradient of active components, improves the dispersibility of active metals on the surface of a carrier, and regulates the interaction between active metals and the carrier, thereby improving the hydrodesulfurization activity and stability of the catalyst.

[0044] When the catalyst prepared by the method of the present invention is used for hydrodesulfurization, it can hydrogenate saturated monoolefins to the maximum extent, and is particularly suitable for oil products with variable sulfur content and diene content. At the same time, it can also meet the requirements of high space speed operation, and the catalyst has excellent hydrodesulfurization performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 is the X-ray photoelectron spectrum of the catalyst in specific example 4.

[0046] Figure 2 This is the HRTEM component distribution diagram of potassium in the catalyst in specific example 4. DETAILED DESCRIPTION

[0047] The present invention is described in detail below by way of examples. It is necessary to point out that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Those skilled in the art in this field can make some non-essential improvements and adjustments to the present invention based on the above content of the present invention.

[0048] Example 1

[0049] The carrier used in the experiment is a clover-shaped γ-Al2O3 carrier with a specific surface area of ​​287m 2 / g, pore volume 0.624cm 3 / g, strength 174N / cm, water absorption 102%.

[0050] (1) First, prepare a potassium hydroxide aqueous solution for pretreatment: prepare 306 ml of 0.2% potassium hydroxide solution;

[0051] (2) Weigh 10 kg of aluminum oxide and add it to a rotary impregnation pot. Use the prepared potassium hydroxide solution to spray the carrier. The spraying time is 3 minutes and the standing time after spraying is 8 minutes.

[0052] (3) Add 2750 g of nickel nitrate to a mixed solution of 5000 ml of ammonia water and 700 ml of ethylenediamine, stir and dissolve, then add 4275 g of ammonium molybdate and 1640 g of ammonium metatungstate and stir and dissolve, then add potassium hydroxide, add ammonia water to adjust the solution volume to 12200 ml, impregnate on the support (2), age for 4.5 h, dry at 100° C. for 4 hours, and calcine at 400° C. for 5 hours to obtain catalyst C1.

[0053] Example 2

[0054] The carrier used in the experiment is a clover-shaped γ-Al2O3 carrier with a specific surface area of ​​245m 2 / g, pore volume 0.631cm 3 / g, strength 159N / cm, water absorption 95%.

[0055] (1) First, prepare a potassium hydroxide aqueous solution for pretreatment: prepare 380 ml of 0.3% potassium hydroxide solution;

[0056] (2) Weigh 10 kg of aluminum oxide and add it to a rotary impregnation pot. Use the prepared potassium hydroxide solution to spray the carrier. The spraying time is 4 minutes and the standing time after spraying is 10 minutes.

[0057] (3) Add 6900 g of cobalt nitrate to a mixed solution of 5200 ml of ammonia water and 450 g of ethylenediaminetetraacetic acid, stir and dissolve, then add 4179 g of ammonium molybdate and 1120 g of nickel acetate and stir and dissolve, then add deionized water to adjust the solution volume to 10900 ml, impregnate on the γ-Al2O3 carrier of (2), age for 5 h, dry at 110°C for 5 h, and calcine at 420°C for 4 h to obtain catalyst C2.

[0058] Example 3

[0059] The carrier used in the experiment is a clover-shaped γ-Al2O3 carrier with a specific surface area of ​​302m 2 / g, pore volume 0.611cm 3 / g, strength 181N / cm, water absorption 92%.

[0060] (1) First, prepare a potassium hydroxide aqueous solution for pretreatment: prepare 460 ml of a 0.5% potassium hydroxide solution;

[0061] (2) Weigh 10 kg of aluminum oxide and add it to a rotary impregnation pot. Use the prepared potassium hydroxide solution to spray the carrier. The spraying time is 5 minutes. The standing time after spraying is 10 minutes.

[0062] (3) 1430 g of cobalt nitrate was added to a mixed solution of 5300 ml of ammonia water and 400 ml of triethylenetetramine, stirred and dissolved, and then 3315 g of ammonium molybdate and 1045 g of nickel nitrate were added and stirred and dissolved, and potassium hydroxide was added. Deionized water was added to adjust the solution volume to 10310 ml, and the solution was impregnated on the γ-Al2O3 carrier of (2), aged for 6 h, dried at 120°C for 4 h, and calcined at 450°C for 4 h to obtain catalyst C3.

[0063] Example 4

[0064] The carrier used in the experiment is a clover-shaped γ-Al2O3 carrier with a specific surface area of ​​295m 2 / g, pore volume 0.641cm 3 / g, strength 212N / cm, water absorption 89%.

[0065] (1) First, prepare a potassium hydroxide aqueous solution for pretreatment: prepare 534 ml of a 0.6% potassium hydroxide solution;

[0066] (2) Weigh 10 kg of aluminum oxide and add it to a rotary impregnation pot. Use the prepared potassium hydroxide solution to spray the carrier. The spraying time is 6 minutes. The standing time after spraying is 15 minutes.

[0067] (3) 1370 g of cobalt acetate was added to a mixed solution of 5500 ml of ammonia water and 480 ml of ethylenediamine, stirred and dissolved, and then 2712 g of ammonium molybdate and 840 g of nickel nitrate were added and stirred and dissolved, and potassium hydroxide was added. Ammonia water was added to adjust the solution volume to 9620 ml, and the solution was impregnated on the γ-Al2O3 carrier of (2), aged for 8 h, dried at 100°C for 6 h, and calcined at 500°C for 4 h to obtain catalyst C4.

[0068] Example 5

[0069] The carrier used in the experiment is a clover-shaped γ-Al2O3 carrier with a specific surface area of ​​261m 2 / g, pore volume 0.641cm 3 / g, strength 168N / cm, water absorption 110%.

[0070] (1) First, prepare a potassium hydroxide aqueous solution for pretreatment: prepare 880 ml of 0.8% potassium hydroxide solution;

[0071] (2) Weigh 10 kg of aluminum oxide and add it to a rotary impregnation pot. Use the prepared potassium hydroxide solution to spray the carrier. The spraying time is 8 minutes and the standing time after spraying is 20 minutes.

[0072] (3) 1240 g of cobalt acetate, 2910 g of ammonium molybdate and 680 g of nickel nitrate were added to a mixed solution of 6000 ml of aqueous ammonia and 500 ml of ethylenediamine, stirred and dissolved, potassium hydroxide was added, and aqueous ammonia was added to adjust the solution volume to 11230 ml, and impregnated on the γ-Al2O3 carrier of (2), aged for 10 h, dried at 110°C for 5 h, and calcined at 520°C for 4 h to obtain catalyst C5.

[0073] Example 6

[0074] The carrier used in the experiment is a clover-shaped γ-Al2O3 carrier with a specific surface area of ​​251m 2 / g, pore volume 0.598cm 3 / g, strength 224N / cm, water absorption 98%.

[0075] (1) First, prepare a potassium hydroxide aqueous solution for pretreatment: prepare 980 ml of a 1.0% potassium hydroxide solution;

[0076] (2) Weigh 10 kg of aluminum oxide and add it to a rotary impregnation pot. Use the prepared potassium hydroxide solution to spray the carrier. The spraying time is 8 minutes and the standing time after spraying is 20 minutes.

[0077] (3) 1145 g of cobalt acetate, 1980 g of ammonium metatungstate and 760 g of nickel nitrate were added to a mixed solution of 5800 ml of aqueous ammonia and 450 ml of ethylenediamine, stirred and dissolved, potassium hydroxide was added, and deionized water was added to adjust the solution volume to 9430 ml. The solution was impregnated on the γ-Al2O3 carrier of (2), aged for 12 h, dried at 100°C for 6 h, and calcined at 550°C for 4 h to obtain catalyst C6.

[0078] Comparative Example 1

[0079] The carrier used in the experiment is a clover-shaped γ-Al2O3 carrier with a specific surface area of ​​287m 2 / g, pore volume 0.624cm 3 / g, strength 174N / cm, water absorption 102%.

[0080] Add 2750g of nickel nitrate to a mixed solution of 5000ml of ammonia water and 700ml of ethylenediamine, stir to dissolve, then add 4275g of ammonium molybdate and 1640g of ammonium metatungstate and stir to dissolve, then add potassium hydroxide, add ammonia water to adjust the solution volume to 12200ml, impregnate on the carrier, age for 4.5h, dry at 100℃ for 4h, and calcine at 400℃ for 5h to obtain catalyst D1.

[0081] Comparative Example 2

[0082] The carrier used in the experiment is a clover-shaped γ-Al2O3 carrier with a specific surface area of ​​245m 2 / g, pore volume 0.631cm 3 / g, strength 159N / cm, water absorption 95%.

[0083] Add 6900 g of cobalt nitrate to a mixed solution of 5200 ml of ammonia water and 450 g of ethylenediaminetetraacetic acid, stir to dissolve, then add 4179 g of ammonium molybdate and 1120 g of nickel acetate and stir to dissolve, then add deionized water to adjust the solution volume to 10900 ml, impregnate on the carrier, age for 5 hours, dry at 110°C for 5 hours, and calcine at 420°C for 4 hours to obtain catalyst D2.

[0084] Comparative Example 3

[0085] The carrier used in the experiment is a clover-shaped γ-Al2O3 carrier with a specific surface area of ​​302m 2 / g, pore volume 0.611cm 3 / g, strength 181N / cm, water absorption 92%.

[0086] 1430 g of cobalt nitrate was added to a mixed solution of 5300 ml of ammonia water and 400 ml of triethylenetetramine, stirred to dissolve, and then 3315 g of ammonium molybdate and 1045 g of nickel nitrate were added and stirred to dissolve, potassium hydroxide was added, and deionized water was added to adjust the solution volume to 10310 ml, impregnated on a carrier, aged for 6 hours, dried at 120°C for 4 hours, and calcined at 450°C for 4 hours to obtain catalyst D3.

[0087] Comparative Example 4

[0088] The carrier used in the experiment is a clover-shaped γ-Al2O3 carrier with a specific surface area of ​​261m 2 / g, pore volume 0.641cm 3 / g, strength 168N / cm, water absorption 110%.

[0089] Add 1240g of cobalt acetate, 2910g of ammonium molybdate and 680g of nickel nitrate to a mixed solution of 6000ml of aqueous ammonia and 500ml of ethylenediamine, stir to dissolve, add potassium hydroxide, add aqueous ammonia to adjust the solution volume to 11230ml, impregnate on the carrier, age for 10h, dry at 110°C for 5h, and calcine at 520°C for 4h to obtain catalyst D4.

[0090] Comparative Example 5

[0091] This comparative example prepared the catalyst according to the method described in Example ZL99113281.5, and the specific steps are as follows:

[0092] The carrier used in the experiment is a clover-shaped γ-Al2O3 carrier with a specific surface area of ​​287m 2 / g, pore volume 0.624cm 3 / g, strength 174N / cm, water absorption 102%.

[0093] Mix 4500g of ammonium metatungstate, 1325g of nickel carbonate, 1775g of molybdenum oxide, 950g of phosphoric acid and 6000ml of deionized water, then heat to 110°C and dissolve for 1 hour, then add 2750g of nickel nitrate, stir and dissolve to obtain a W-Mo-Ni-P co-impregnation solution, dilute to 20000ml with deionized water, impregnate 22g of the calcined carrier with the above impregnation solution at room temperature, dry at 150°C for 2h, calcine at 480°C for 2h, then impregnate with the above impregnation solution at room temperature, and then dry and calcine to obtain the final catalyst D5.

[0094] Table 1 Potassium oxide mass content in catalyst

[0095] Potassium oxide wt% Example 1 0.32 Example 2 2.01 Example 3 1.37 Example 4 1.25 Example 5 2.54 Example 6 0.79 Comparative Example 1 0.32 Comparative Example 2 2.01 Comparative Example 3 1.37 Comparative Example 4 2.54

[0096] The element distribution analysis of the catalyst was performed by SEM to characterize the distribution of active components on the catalyst. The content of active components at different positions in the catalyst is shown in the following table.

[0097] Table 2 The percentage of active component metal content in different positions of the catalyst to the total content of active components (%)

[0098] Center to 1 / 4 radius 1 / 4 to 1 / 2 radius 1 / 2 to 3 / 4 radius 3 / 4 radius to surface Example 1 3.1 10.1 7.9 78.9 Example 2 2.6 8.4 8.7 80.3 Example 3 2.4 4.2 12.8 80.6 Example 4 1.8 7.8 10.5 79.9 Example 5 1.5 5.1 11.4 82 Example 6 1.3 6.4 15.8 76.5 Comparative Example 1 7.1 15.6 24.8 52.5 Comparative Example 2 5.4 14.2 31.4 49 Comparative Example 3 6.7 11.7 29.1 52.5 Comparative Example 4 4.9 16.5 20.5 58.1

[0099] The catalysts C5 and D4 prepared above were evaluated for 300 hours respectively, using the first stage hydrogenation product of pyrolysis gasoline as the raw material. The properties of the raw material are shown in Table 3. The catalyst evaluation was carried out on a 250ml adiabatic bed hydrogenation reaction device. The iodine value and sulfur content of the product were sampled and analyzed every 12 hours. The average data of the catalyst evaluation for 300 hours is shown in Table 4.

[0100] The pre-sulfurization conditions of the catalyst are as follows: add carbon disulfide to naphtha to prepare sulfurized oil (sulfur content 1000μg / g), pass hydrogen at a pressure of 2.8MPa, raise the catalyst bed temperature to 240°C, start feeding sulfurized oil, continue to raise the temperature to 280°C, maintain for 20 hours, then cool down to 240°C, and the sulfurization is completed.

[0101] Evaluation conditions: reaction pressure 2.6MPa, inlet temperature 240℃, fresh crude oil volume space velocity 2.5h -1 , based on fresh oil, the volume ratio of hydrogen to oil is 300:1.

[0102] Table 3 Hydrogenation feedstock index

[0103]

[0104] Table 4 Average data of catalyst C5 and D4 evaluated over 300 hours

[0105]

[0106] Table 5 Average data of catalyst C1, D1, D5 after 300 hours of evaluation

[0107]

[0108] The catalysts C1, D1 and D5 prepared above were subjected to 300-hour hydrogenation evaluation, respectively, using diesel as the raw material. The raw material properties are shown in Table 3. The catalyst evaluation was carried out on a 250ml adiabatic bed hydrogenation reaction device. The nitrogen and sulfur content of the products were sampled and analyzed every 12 hours. The average data of the catalyst 300-hour evaluation is shown in Table 6.

[0109] The pre-sulfurization conditions of the catalyst are as follows: add carbon disulfide to naphtha to prepare sulfurized oil (sulfur content 1000μg / g), pass hydrogen at a pressure of 2.8MPa, raise the catalyst bed temperature to 240℃, start feeding sulfurized oil, continue to raise the temperature to 300℃, maintain for 24 hours, then cool to 280℃, and the sulfurization is completed.

[0110] Evaluation conditions: reaction pressure 2.8MPa, inlet temperature 280℃, fresh crude oil volume space velocity 2.0h -1 , based on fresh oil, the volume ratio of hydrogen to oil is 300:1.

[0111] From the evaluation results in Table 4, it can be seen that the catalyst preparation method provided by the present invention can improve the dispersion of the active components of the catalyst, so that the catalyst has better hydrogenation activity.

[0112] From the evaluation results in Table 5, it can be seen that the catalyst prepared by the catalyst preparation method provided by the present invention has higher hydrodesulfurization and denitrification activities.

[0113] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, technicians familiar with the field may make various corresponding changes and deformations based on the present invention, but these corresponding changes and deformations should all fall within the scope of protection of the claims of the present invention.

Claims

1. A method for preparing a hydrorefining catalyst, wherein the catalyst carrier is a high temperature resistant inorganic oxide, characterized in that: The catalyst contains potassium, part of which is introduced by pre-spraying the carrier; part of the potassium is introduced by impregnating the carrier with an active component impregnation solution containing potassium. After spraying, the carrier needs to be aged before being impregnated with the active component solution. The spraying step is before the active component loading, and the spraying completion time is 1min~20min.

2. The method for preparing a hydrotreating catalyst according to claim 1, characterized in that: The high temperature resistant inorganic oxide is one or more of aluminum oxide, silicon oxide, titanium oxide and zirconium oxide.

3. The method for preparing a hydrotreating catalyst according to claim 2, characterized in that: The high temperature resistant inorganic oxide is aluminum oxide.

4. The method for preparing a hydrotreating catalyst according to claim 1, characterized in that: The water absorption rate of the carrier is 80% to 120%.

5. The method for preparing a hydrotreating catalyst according to claim 4, characterized in that: The water absorption rate of the carrier is 85% to 110%.

6. The method for preparing a hydrotreating catalyst according to claim 1, characterized in that: The carrier is pre-sprayed with potassium hydroxide solution, the concentration of potassium hydroxide is 0.1%~5%, the spraying amount of potassium hydroxide solution required for each gram of carrier is [carrier mass × water absorption rate × (1%~20%)] ml, and the potassium oxide content in the catalyst is 0.3wt%~5wt%.

7. The method for preparing a hydrotreating catalyst according to claim 1, characterized in that: The concentration of potassium hydroxide is 0.5%~1%; the content of potassium oxide in the catalyst is 0.5wt%~2.5wt%.

8. The method for preparing a hydrotreating catalyst according to claim 6, characterized in that: The preparation method of potassium hydroxide solution is: dissolve potassium hydroxide in deionized water, and the pH value of the prepared potassium hydroxide solution is 12.2~13.

5.

9. The method for preparing a hydrotreating catalyst according to claim 1, characterized in that: After the carrier is aged after spraying, the catalyst preparation is directly carried out without drying and calcination, and the aging time is 5min~30min.

10. The method for preparing a hydrotreating catalyst according to claim 9, characterized in that: The aging time is 10min~20min.

11. The method for preparing a hydrotreating catalyst according to claim 1, characterized in that: The spraying completion time is 3min~10min.

12. The method for preparing a hydrotreating catalyst according to claim 1, characterized in that: The preparation method of the active component impregnation solution containing potassium is as follows: potassium hydroxide, ammonia water, a polyamine complexing agent and deionized water are mixed to prepare a composite solvent, and the salt containing the active component is added into the composite solvent.

13. The method for preparing a hydrotreating catalyst according to claim 12, characterized in that: The volume of potassium-containing active component impregnation solution required for each gram of carrier is [carrier mass × 1.05 × (1-percentage of potassium hydroxide solution added) × water absorption rate of carrier] ml~[carrier mass × 1.25 × (1-percentage of potassium hydroxide solution added) × water absorption rate of carrier] ml.

14. The method for preparing a hydrotreating catalyst according to claim 13, characterized in that: The volume of composite impregnation solution required for each gram of carrier is [carrier mass × 1.1 × (1-percentage of potassium hydroxide solution added) × water absorption rate of carrier] ml~[carrier mass × 1.2 × (1-percentage of potassium hydroxide solution added) × water absorption rate of carrier] ml.

15. The method for preparing a hydrotreating catalyst according to claim 12, characterized in that: The polyamine complexing agent is a C2-C7 compound containing one or more NH groups. The amount of the polyamine complexing agent added is 3-9% based on 100% of the volume of the active component impregnation solution containing potassium.

16. The method for preparing a hydrotreating catalyst according to claim 12, characterized in that: The polyamine complexing agent is ethylenediaminetetraacetic acid, a primary amine, a secondary amine or a tertiary amine.

17. The method for preparing a hydrotreating catalyst according to claim 12, characterized in that: The polyamine complexing agent is ethylenediamine.