Preform solder composition, solder sheet and preparation method
By mixing the solder powder with flux and adhesive before preforming, the problem of difficult molding of high-temperature soft solder and high-temperature hard solder is solved. Tin-silver-copper or tin-lead based solder waste is used to achieve efficient molding. and cost reduction, suitable for the field of microelectronics.
Patent Information
- Application Number
- CN202211709913.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-29
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2042-12-29
AI Technical Summary
It is difficult to directly roll and shape high-temperature soft solder or high-temperature hard solder with the existing solder sheet production process, and the waste or returned materials generated during the production process of tin-silver-copper or tin-lead solder cannot be effectively utilized, resulting in uneven flux distribution. Affect the quality of welding pieces.
A preformed solder composition is used, including solder powder, flux and adhesive. The solder powder is made into powder and mixed with flux and adhesive before preforming. It is suitable for brittle high-temperature solder. Or use high-temperature brazing materials, including scraps of tin-silver-copper or tin-lead brazing materials, to prepare regular or irregular-shaped soldering pieces using rolling or extrusion molding processes.
The effective molding of high-temperature soft solder and high-temperature hard solder is achieved. The yield of solder sheets reaches more than 90%. The welding quality is comparable to that of commercially available solder sheets, and the production cost is reduced by at least 30%.
Smart Images

Figure CN115846930B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of welding materials, and in particular relates to a preformed solder composition, a welding sheet and a preparation method. Background Art
[0002] Solder is a metal material used to fill the weld during welding. It has been widely used in interconnection and sealing in various fields. However, with the development of industrial technology, the requirements for the technical indicators and economic efficiency of solder are becoming higher and higher. Take the field of microelectronics as an example. With the development of electronic assembly technology, electronic components are becoming more and more miniaturized and personalized, and electronic products are developing towards ultra-high power and ultra-high integration. Therefore, the process requirements for welding and filling are becoming more and more special.
[0003] For example, existing solder bars, solder wires, solder balls, solder pastes, etc. cannot further meet the requirements, especially in terms of ease of use and economy. Preformed solders are developed to meet the new requirements of the above technological developments for solders, because preformed solders can be made into specific shapes and specifications, as well as precision welds with different surface morphologies according to the different requirements of welding electronic components, to meet the welding requirements of small tolerance precision quantification or specified weld thickness (height) that traditional welds cannot meet. This technology has now begun to be widely used in printed circuit board assembly, chip connection, optical fiber core, connectors, terminal equipment and electronic component assembly.
[0004] At present, the production of solder sheets with flux at home and abroad mostly adopts the process of alloy melting and casting → slab making → rolling → punching → cleaning and drying → flux coating → drying and cooling → packaging, or the flux is placed in the solder core before the sheet is rolled into shape. However, these two processes are not suitable for high-temperature soft solder or high-temperature hard solder that is brittle and difficult to be directly rolled into shape, and the waste or return materials generated in the production process of tin-silver-copper or tin-lead solder cannot be well utilized. When producing other special-shaped solder sheets, the flux distribution is easily uneven during the molding process, resulting in a decrease in the quality of the solder sheet. Summary of the invention
[0005] The technical purpose of the present invention is to at least solve the problems existing in the existing solder sheet production, such as being unsuitable for high-temperature soft solder or high-temperature hard solder that is brittle and difficult to be directly rolled into shape, or being unable to make good use of waste or returned materials generated in the production process of tin-silver-copper or tin-lead solder, or being prone to uneven distribution of flux during the molding process when producing other special-shaped solder sheets, which leads to a decrease in the quality of the solder sheet.
[0006] This purpose is achieved through the following technical solutions:
[0007] In a first aspect, the present invention provides a preform solder composition, the composition comprising the following raw material components in percentage by weight:
[0008] Solder powder: 50wt%~94wt%;
[0009] Flux: 5wt%~40wt%;
[0010] Adhesive: 1wt%~10wt%;
[0011] Wherein, the solder powder is selected from any one of medium-temperature solder and waste materials used to produce the medium-temperature solder, high-temperature solder, and high-temperature hard solder;
[0012] The melting temperature of the medium temperature solder is 170-230°C;
[0013] The melting temperature of the high temperature solder is ≥260°C;
[0014] The melting temperature of the high-temperature brazing filler metal is ≥800°C.
[0015] In some embodiments of the present invention, the medium temperature solder comprises a solder having a melting temperature of 175 to 185°C or a solder having a melting temperature of 210 to 230°C;
[0016] In some embodiments of the present invention, the solder having a melting temperature of 175-185° C. is preferably a tin-lead solder, and the tin-lead solder comprises one or two or more of SnPb37, SnPb40, SnPb36Ag2 or SnPb36.6Ag0.4.
[0017] In some embodiments of the present invention, the solder having a melting temperature of 210 to 230°C is preferably a lead-free solder, and the lead-free solder comprises one or two or more of SnAg3.5, SnAg3.0Cu0.5, SnAg3.8Cu0.7, SnAg3.9Cu0.6, SnAg4.0Cu0.5, SnAg0.3Cu0.7, SnAg1.0Cu0.5, SnAg3.0Cu0.5Ni0.05 or SnCu0.7.
[0018] In some embodiments of the present invention, the medium-temperature solder and the waste material thereof are made of the same material but have different particle sizes, wherein the particle size of the waste material does not meet the finished product requirements of the medium-temperature solder.
[0019] Specifically, when producing tin-lead and lead-free solders, taking the production of T4 solder powder as an example, the solder itself has a particle size in the range of 20 to 38 μm, and the solder powder that does not meet this particle size range is waste. Taking the production of T3 solder powder as an example, the solder itself has a particle size in the range of 25 to 45 μm, and the solder powder that does not meet this particle size range is waste. Taking the production of T5 solder powder as an example, the solder itself has a particle size in the range of 15 to 25 μm, and the solder powder that does not meet this particle size range is waste. The waste can be reused, which is beneficial to reducing production costs.
[0020] In some embodiments of the present invention, the melting temperature of the high temperature solder is 260-380°C;
[0021] In some embodiments of the present invention, the high temperature solder comprises a solder having a melting temperature of 260 to 290°C or a solder having a melting temperature of 280 to 380°C;
[0022] Wherein, the solder with a melting temperature of 260-290° C. is a bismuth-based solder; and the bismuth-based solder comprises one, two or three of BiAg2.5, BiAg10 or BiSb10Ag2.5;
[0023] The solder with a melting temperature of 280-380° C. is a gold-based solder; and the gold-based solder includes one, two or three of AuSn20, AuGe12 and AuSi2.
[0024] In some embodiments of the present invention, the high temperature brazing filler metal is a commonly used stainless steel brazing filler metal.
[0025] In some embodiments of the present invention, the commonly used stainless steel solder includes at least one of BNi5 and BNi7.
[0026] The high-temperature soft solder and the high-temperature hard solder are usually brittle and generally difficult to be directly rolled or formed. In particular, for special shapes that need to be made, the conventional process is likely to cause uneven distribution of flux and lead to a decrease in the quality of the solder sheet. The present invention first makes this type of solder into a powder, mixes the powder with flux and adhesive, and then pre-forms it. This not only solves the problem caused by the uneven distribution of the components, but also makes it easy to prepare into the required special shapes.
[0027] In some embodiments of the present invention, the solder powder is a 200-mesh sieve powder.
[0028] In some embodiments of the present invention, the composition further comprises 0.1‰wt~5‰wt of uniformly sized infusible particles, the particle size of which is larger than the particle size of the solder powder, and preferably, the particle size of the infusible particles is more than three times the particle size of the solder powder. The infusible particles will not collapse due to melting during the welding process, and the use of infusible particles with a uniform particle size distribution is conducive to ensuring the same or similar height during the welding process, further improving the welding performance.
[0029] In some embodiments of the present invention, the composition comprises the following raw material components in the following mass percentages:
[0030] Solder powder: 54wt%~85wt%;
[0031] Flux: 10wt%~40wt%;
[0032] Adhesive: 3wt%~7wt%;
[0033] Unmelted particles: 0.5‰wt~5‰wt;
[0034] Wherein, the infusible particles are one or two or more of metal nickel, metal silver, and resin particles.
[0035] Wherein, the resin particles are commercially available spherical polyethylene particles.
[0036] In some embodiments of the present invention, the soldering flux is any form of soldering flux commonly used in the art, and the soldering flux plays a role of deoxidation and decontamination during the welding process.
[0037] In some embodiments of the present invention, the adhesive is a thermoplastic adhesive, and the thermoplastic adhesive includes a polyurethane adhesive or a polyethylene glycol adhesive, and the molecular weight of the polyurethane adhesive or the polyethylene glycol adhesive is 600 to 6000. The adhesive with this feature can achieve fast drying and curing during the solder sheet preforming process, thereby improving the formability and strength of the solder sheet.
[0038] In a second aspect, the present invention provides a preformed solder sheet, wherein the solder sheet is formed by rolling or extrusion using the preformed solder composition of the first aspect, and the solder sheet has a regular shape or an irregular shape.
[0039] In some embodiments of the present invention, the raw material components in the preform solder composition are mixed to obtain a mixture, and the mixture is rolled or extruded at 60-150° C. to obtain the solder sheet.
[0040] The preformed solder sheet prepared by the present invention is suitable for the field of microelectronic interconnection, such as chip welding and the like.
[0041] The beneficial effects of the technical solution disclosed in the present invention are mainly reflected in the following:
[0042] The preformed solder provided by the present invention includes high-temperature soft solder or high-temperature hard solder that is brittle and difficult to be directly rolled and formed, and may also include waste or returned materials generated in the production process of tin-silver-copper or tin-lead solder. This type of solder is suitable for various conventional forming processes and is easy to form various regular shapes or irregular special-shaped solder pieces, with a yield rate of more than 90%. In addition, the welding quality of the solder piece is comparable to that of the commercially available preformed solder piece, and the production cost is greatly reduced, for example, at least about 30% of the cost is saved. This type of preformed solder has good application prospects in the field of microelectronic interconnection. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Various other advantages and benefits will become apparent to those of ordinary skill in the art by reading the detailed description of the preferred embodiments below. The accompanying drawings are only for the purpose of illustrating the preferred embodiments and are not to be considered as limiting the present invention. Moreover, the same reference numerals are used throughout the accompanying drawings to represent the same components. In the accompanying drawings:
[0044] Figure 1 The schematic diagram of the size structure of the preformed solder sheet prepared according to Example 1 of the present invention is shown;
[0045] Figure 2 The schematic diagram of the size structure of the preformed welding sheet prepared according to Example 4 of the present invention is shown;
[0046] Figure 3 The schematic diagram of the positional relationship of each component in the welding process is shown schematically;
[0047] Figure 4 Schematically showing a post-welding X-ray interface void test photograph of a preformed solder sheet prepared according to Example 1 of the present invention;
[0048] Figure 5 Schematically shows a post-weld X-ray interface void test photograph of a commercially available SnAgCu preform;
[0049] Figure 6 The schematic diagram of the size structure of the preformed solder sheet prepared according to Example 7 of the present invention is shown;
[0050] The reference numerals in the accompanying drawings represent the following:
[0051] 1. Chip; 2. Preformed solder sheet; 3. Substrate; 4. Pad; DETAILED DESCRIPTION
[0052] The existing technology for producing preformed solder sheets has the following problems: it is not suitable for high-temperature soft solder and high-temperature hard solder that are brittle and difficult to be directly rolled and formed, such solders include bismuth-based solder, gold-based solder, or commonly used stainless steel solder; waste or return materials generated in the production process of tin-silver-copper or tin-lead solder cannot be well utilized; for other special-shaped solder sheets, the molding process is prone to uneven distribution of flux, resulting in reduced quality of the solder sheet, etc.
[0053] In order to solve the above technical problems, the present invention provides a preformed solder composition, a solder sheet and a preparation method. This type of solder includes high-temperature soft solder or high-temperature hard solder that is brittle and difficult to be directly rolled and formed, and may also include waste or return materials generated in the production process of tin-silver-copper or tin-lead solders, and is suitable for various conventional molding processes, and is easy to form various regular shapes or irregular special-shaped solder sheets, wherein the yield is above 90%. In addition, the welding quality of the solder sheet is comparable to that of the commercially available preformed solder sheets, and the production cost is greatly reduced, for example, at least about 30% of the cost is saved. This type of preformed solder has good application prospects in the field of microelectronic interconnection.
[0054] In order to achieve the above technical effects, the first aspect of the present invention is to disclose a preform solder composition, which comprises the following raw material components in percentage by mass:
[0055] Solder powder: 50wt%~94wt%;
[0056] Flux: 5wt%~40wt%;
[0057] Adhesive: 1wt%~10wt%;
[0058] Wherein, the solder powder is selected from any one of medium-temperature solder and waste materials used to produce the medium-temperature solder, high-temperature solder, and high-temperature hard solder;
[0059] The melting temperature of the medium temperature solder is 170-230°C;
[0060] The melting temperature of the high temperature solder is ≥260°C;
[0061] The high temperature brazing filler metal is ≥800°C.
[0062] The present invention solves the technical problem that various high-temperature soft solders or high-temperature hard solders that are brittle and difficult to be directly rolled and formed are difficult to be preformed by first mixing them with flux and adhesive, thereby solving the technical problem that such solders are difficult to be directly rolled and formed or formed into special-shaped solder sheets. At the same time, for medium-temperature soft solders, waste scraps that do not meet the requirements are easily generated during the production process. The present invention can reuse such waste scraps, which is beneficial to reducing production costs.
[0063] In some embodiments, the solder powder is a 200-mesh sieve powder, wherein 200 mesh corresponds to 75 μm, that is, the particle size of the solder powder is less than 75 μm. After the solder powder meeting this particle size distribution is fully mixed with the flux and the adhesive, it is not only conducive to preforming into sheets, but also conducive to improving the uniformity of the performance of the solder sheet.
[0064] In some embodiments, the medium temperature solder comprises a solder having a melting temperature of 175-185°C or a solder having a melting temperature of 210-230°C.
[0065] Exemplarily, the solder having a melting temperature of 175-185° C. is preferably a tin-lead solder.
[0066] The tin-lead solder comprises one or two or more of SnPb37, SnPb40, SnPb36Ag2 or SnPb36.6Ag0.4.
[0067] Exemplarily, the solder having a melting temperature of 210-230° C. is preferably a lead-free solder.
[0068] Wherein, the lead-free solder contains one or two or more of SnAg3.5, SnAg3.0Cu0.5, SnAg3.8Cu0.7, SnAg3.9Cu0.6, SnAg4.0Cu0.5, SnAg0.3Cu0.7, SnAg1.0Cu0.5, SnAg3.0Cu0.5Ni0.05 or SnCu0.7.
[0069] In some embodiments, the medium-temperature solder and the waste material thereof are made of the same material but have different particle sizes, wherein the particle size of the waste material does not meet the finished product requirements of the medium-temperature solder.
[0070] Specifically, when producing tin-lead and lead-free solders, taking the production of T4 solder powder as an example, the solder itself has a particle size in the range of 20 to 38 μm, and the solder powder that does not meet this particle size range is waste. Taking the production of T3 solder powder as an example, the solder itself has a particle size in the range of 25 to 45 μm, and the solder powder that does not meet this particle size range is waste. Taking the production of T5 solder powder as an example, the solder itself has a particle size in the range of 15 to 25 μm, and the solder powder that does not meet this particle size range is waste. The waste can be reused, which is beneficial to reducing production costs.
[0071] In some embodiments, the melting temperature of the high temperature solder is 260-380°C.
[0072] In some embodiments, the high temperature solder comprises a solder having a melting temperature of 260-290°C or a solder having a melting temperature of 280-380°C.
[0073] Exemplarily, the solder having a melting temperature of 260 to 290° C. is a bismuth-based solder; wherein the bismuth-based solder comprises one, two or three of BiAg2.5, BiAg10 or BiSb10Ag2.5;
[0074] Exemplarily, the solder having a melting temperature of 280 to 380° C. is a gold-based solder; the gold-based solder comprises one, two or three of AuSn20, AuGe12 and AuSi2.
[0075] In some embodiments, the high temperature brazing filler metal is a common stainless steel brazing filler metal.
[0076] In some embodiments, the commonly used stainless steel solder includes at least one of BNi5 and BNi7.
[0077] In some embodiments of the present invention, the composition further comprises 0.1‰wt~5‰wt of uniformly sized infusible particles, the particle size of which is larger than the particle size of the solder powder, and preferably, the particle size of the infusible particles is more than three times the particle size of the solder powder. The infusible particles will not collapse due to melting during the welding process, and the use of infusible particles with a uniform particle size distribution is conducive to ensuring the same or similar height during the welding process, further improving the welding performance.
[0078] In some embodiments, the composition comprises the following weight percentages of each raw material component:
[0079] Solder powder: 54wt%~85wt%;
[0080] Flux: 10wt%~40wt%;
[0081] Adhesive: 3wt%~7wt%;
[0082] Infusible particles: 0.5wt‰~5wt‰;
[0083] Wherein, the infusible particles are one or two or more of metal nickel, metal silver, and resin particles.
[0084] Wherein, the resin particles are commercially available spherical polyethylene particles.
[0085] Exemplarily, the composition comprises the following raw material components in the following mass percentages:
[0086] Solder powder: 54.5wt%;
[0087] Flux: 40wt%;
[0088] Adhesive: 5wt%;
[0089] Unmelted particles: 0.5wt%.
[0090] Exemplarily, the composition comprises the following raw material components in the following mass percentages:
[0091] Solder powder: 79.9wt%;
[0092] Flux: 15wt%;
[0093] Adhesive: 5wt%;
[0094] Unmelted particles: 0.1wt%.
[0095] Exemplarily, the composition comprises the following raw material components in the following mass percentages:
[0096] Solder powder: 85wt%;
[0097] Flux: 10wt%;
[0098] Adhesive: 5wt%.
[0099] In some embodiments, the soldering flux is any form of soldering flux commonly used in the art, which is not listed in detail in the present invention. The soldering flux plays a role in deoxidation and decontamination during the welding process.
[0100] In some embodiments, the adhesive is a thermoplastic adhesive, and the thermoplastic adhesive includes a polyurethane adhesive or a polyethylene glycol adhesive, and the molecular weight of the polyurethane adhesive or the polyethylene glycol adhesive is 600 to 6000. The adhesive with this feature can achieve fast drying and curing during the solder sheet preforming process, thereby improving the formability and strength of the solder sheet.
[0101] Exemplarily, the molecular weight of the thermoplastic adhesive may be any one of 600, 700, 800, 900, 1000, 1200, 1400, 1600, 1800, 2000, 2200, 2400, 2600, 2800, 3000, 3200, 3400, 3600, 3800, 4000, 4200, 4400, 4600, 4800, 5000, 5200, 5400, 5600, 5800, 6000 or any one satisfying the above range, and the unit is Dalton.
[0102] In order to achieve the above technical effects, the second aspect of the present invention discloses a preformed solder sheet, which is formed by rolling or extrusion using the preformed solder composition described in the first aspect, and the solder sheet has a regular shape or an irregular shape.
[0103] In some embodiments, the raw material components in the preform solder composition are mixed to obtain a mixture, and the mixture is calendered or extruded at 60-150° C. to obtain the solder sheet.
[0104] The exemplary embodiments of the present disclosure will be described in more detail below with reference to the accompanying drawings. Although the exemplary embodiments of the present disclosure are shown in the accompanying drawings, it should be understood that the present disclosure can be implemented in various forms and should not be limited by the embodiments described herein. On the contrary, these embodiments are provided in order to enable a more thorough understanding of the present disclosure and to fully convey the scope of the present disclosure to those skilled in the art. Among them, the models and manufacturers of the various chemical raw materials used in the following embodiments are not subject to special limiting requirements.
[0105] Example 1
[0106] A method for preparing a preformed solder sheet is disclosed, comprising the following preparation steps:
[0107] (1) Weigh 50 g of Ni particles with a particle size of 500 μm, 4 kg of halogen-free flux, 500 g of polyurethane thermoplastic adhesive with a molecular weight of 1000, and the remainder of SnAg3.0Cu0.5 recycled powder, a total of 10 kg;
[0108] (2) placing the raw materials of step (1) in a stainless steel barrel and stirring to obtain a viscous paste, transferring the paste to the loading barrel of a roller mill, adjusting the roller gap to 0.76 mm, heating the rollers to 125° C., and adjusting the roller speed to 0.5 r / min to ensure that the paste has a certain shape retention after rolling;
[0109] (3) After cooling, the blanking size is 2.03mm×1.27mm×0.76mm (a×b×c). Figure 1 The rectangular preforms shown are packaged and the yield is about 98%.
[0110] Example 2
[0111] A method for preparing a preformed solder sheet is disclosed, and the difference between this embodiment and embodiment 1 is that the SnAg3.0Cu0.5 return powder is replaced with SnAg3.0Cu0.5 solder powder, and the other parts remain the same. The yield is about 98%.
[0112] Example 3
[0113] A method for preparing a preformed solder sheet is disclosed, and the difference between this embodiment and embodiment 1 is that the halogen-free soldering flux is 2 kg, and the other parts remain the same, and the yield is about 98%.
[0114] Example 4
[0115] A method for preparing a preformed solder sheet is disclosed, comprising the following preparation steps:
[0116] (1) Weigh 10 g of pure Ag particles with a particle size of 760 μm, 500 g of rosin-based flux, 100 g of polyethylene glycol thermoplastic adhesive with a molecular weight of 1000, and the remainder of SnPb36Ag2 reflow solder powder, a total of 10 kg;
[0117] (2) placing the raw materials of step (1) in a stainless steel barrel, controlling the temperature to 150° C., stirring to obtain a viscous paste, transferring the paste to the feeding barrel of an extruder, adjusting the outlet diameter of the extruder to 0.5 mm, adjusting the temperature of the extruder to 150° C., and adjusting the extrusion speed to 2 mm / min, ensuring that the viscous paste has a certain shape retention after extrusion;
[0118] (3) After cooling, cut the columnar solder into standard size like Figure 2 The cylindrical preforms shown are packaged and the yield is 98%.
[0119] The soldering sheets prepared in Examples 1 to 4 are placed Figure 3 The corresponding pad position is then placed in a reflow oven with a peak furnace temperature set at 265°C. After the SnAgCu preform solder is melted, the whole is cooled to form a solid interconnection. The X-ray interface void test photo of the solder sheet prepared in Example 1 after soldering is shown in FIG. Figure 4 As shown, in order to reflect the welding quality of the welding sheet of the present invention, the present invention also adopts the same welding method as above using the commercially available SnAgCu preformed welding sheet, and the obtained X-ray interface void test photos after welding are as shown in Figure 5 As shown, combined Figure 4 , Figure 5 It can be seen that the welding quality of the welding piece designed by the present invention is comparable to that of commercially available products, but the cost is reduced by more than 30%.
[0120] The welding quality of the welding sheets obtained in Example 2, Example 3 and Example 4 is equivalent to that in Example 1.
[0121] For other tin-lead solders, such as SnPb37, SnPb40 or SnPb36.6Ag0.4, or lead-free solders, such as SnAg3.5, SnAg3.8Cu0.7, SnAg3.9Cu0.6, SnAg4.0Cu0.5, SnAg0.3Cu0.7, SnAg1.0Cu0.5, SnAg3.0Cu0.5Ni0.05 or SnCu0.7, the above-mentioned molding method can be used to prepare solder sheets with various regular or irregular shapes, which will not be elaborated in the present invention.
[0122] Example 5
[0123] A method for preparing a preformed solder sheet is disclosed, comprising the following preparation steps:
[0124] (1) Weigh 10 g of spherical polyethylene particles with a particle size of 300 μm, 1.5 kg of halogen-free flux, 0.5 kg of polyurethane thermoplastic adhesive with a molecular weight of 600, and the remainder of BiAg10 solder powder, a total of 10 kg;
[0125] (2) placing the raw materials of step (1) in a stainless steel barrel, controlling the temperature to 60° C., stirring to obtain a viscous paste, transferring the paste to the loading barrel of a roller mill, adjusting the roller gap to 0.4 mm, raising the temperature of the roller to 60° C., and adjusting the roller speed to 1.0 r / min to ensure that the paste has a certain shape retention after rolling;
[0126] (3) After cooling, the blanking size is The round gasket-shaped preformed solder pieces are packaged and the yield rate is about 95%.
[0127] In addition, other bismuth-based solders, such as BiAg2.5, BiSb10Ag2.5, etc., can be made into solder sheets with regular or irregular shapes by using the above-mentioned molding method, which will not be elaborated in the present invention.
[0128] Example 6
[0129] A method for preparing a preformed solder sheet is disclosed, which differs from Example 5 in that BiAg10 solder powder is replaced with AuSn20 solder powder, and the rest remain the same, and the yield is about 98%.
[0130] At the same time, other gold-based solders, such as BiAg2.5, BiSb10Ag2.5, etc., can also be made into solder sheets with various regular or irregular shapes by using the above-mentioned molding method, which will not be elaborated in the present invention.
[0131] Example 7
[0132] A method for preparing a preformed solder sheet is disclosed, comprising the following preparation steps:
[0133] (1) Weigh 8.5 kg of BNi7 high-temperature brazing filler metal powder, 1 kg of fluorinated boric acid-containing flux, and 0.5 kg of a polyurethane thermoplastic adhesive with a molecular weight of 6000, a total of 10 kg;
[0134] (2) placing the raw materials of step (1) in a stainless steel barrel, controlling the temperature to 60° C., stirring to obtain a viscous paste, transferring the paste to the feeding barrel of an extruder, adjusting the outlet of the extruder to a ring-slit type, the outer diameter of the ring-slit die to 5 mm, and the seam width to 1 mm; then adjusting the extruder to 60° C., adjusting the extrusion speed to 0.5 mm / min, and ensuring that the paste has a certain shape retention after extrusion;
[0135] (3) After cooling, the columnar solder is laser cut into standard size like Figure 6 The barrel-shaped preforms shown are packaged and the yield is about 95%.
[0136] Example 8
[0137] A method for preparing a preformed solder sheet is disclosed, which differs from Example 7 in that BNi7 is replaced by BNi5, and the yield is about 95%.
[0138] The advantage of the solder sheet forming process disclosed in Example 5, Example 6, Example 7, and Example 8 is that it can easily realize the preparation of preformed solders of specific shapes, specifications and sizes, and the yield rate is above 90%. However, it is difficult to prepare preformed solders with shapes and specifications that meet the requirements using traditional metal processing methods due to the poor plasticity of the material, especially for thin-walled barrel-shaped or special-shaped products, which is almost impossible to achieve. In addition, the flux in the preformed solders in the above embodiments is evenly distributed, and the welding quality is high.
[0139] In summary, the preformed solder provided by the present invention is easy to form various regular or irregular shaped solder pieces while saving costs, and has good application prospects in the field of microelectronic interconnection, such as chip welding.
[0140] It should be understood that the terms used in the text are only for the purpose of describing specific example embodiments, and are not intended to be limiting. Unless the context clearly indicates otherwise, the singular forms "one", "an" and "said" as used in the text may also be meant to include plural forms. The terms "include", "comprise", "contain", and "have" are inclusive, and therefore specify the existence of stated features, steps, operations, elements and / or parts, but do not exclude the existence or addition of one or more other features, steps, operations, elements, parts, and / or combinations thereof. The method steps, processes, and operations described herein are not interpreted as necessarily requiring them to be performed in the specific order described or illustrated, unless the execution order is clearly indicated. It should also be understood that additional or alternative steps may be used.
[0141] The above is only a preferred specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the protection scope of the claims.
Claims
1. A preform solder composition, characterized in that The composition comprises the following raw material components in percentage by weight: Solder powder: 50wt%~94wt%; Flux: 5wt%~40wt%; Adhesive: 1wt%~10wt%; Wherein, the solder powder is selected from any one of medium-temperature solder, waste material used to produce the medium-temperature solder, and high-temperature solder; The melting temperature of the medium temperature solder is 170-230°C; The melting temperature of the high temperature solder is ≥260°C; The adhesive comprises a polyurethane adhesive or a polyethylene glycol adhesive, and the molecular weight of the polyurethane adhesive or the polyethylene glycol adhesive is 600 to 6000; The composition further comprises infusible particles with uniform particle size distribution, wherein the particle size of the infusible particles is larger than the particle size of the solder powder; The infusible particles are one, two or three of metal nickel, metal silver and resin particles, and the resin particles are commercially available spherical polyethylene particles.
2. The composition according to claim 1, characterized in that The medium-temperature solder includes a solder having a melting temperature of 175 to 185°C or a solder having a melting temperature of 210 to 230°C.
3. The composition according to claim 2, characterized in that The solder with a melting temperature of 175-185° C. is a tin-lead solder, and the tin-lead solder includes one or two or more of SnPb37, SnPb40, SnPb36Ag2 or SnPb36.6Ag0.4; And / or; the solder having a melting temperature of 210-230°C is a lead-free solder, and the lead-free solder contains one or two or more of SnAg3.5, SnAg3.0Cu0.5, SnAg3.8Cu0.7, SnAg3.9Cu0.6, SnAg4.0Cu0.5, SnAg0.3Cu0.7, SnAg1.0Cu0.5, SnAg3.0Cu0.5Ni0.05 or SnCu0.
7.
4. The composition according to claim 1, characterized in that The melting temperature of the high temperature solder is 260-380°C.
5. The composition according to claim 4, characterized in that The high temperature solder includes a solder having a melting temperature of 260 to 290°C or a solder having a melting temperature of 280 to 380°C; Wherein, the solder with a melting temperature of 260-290° C. is a bismuth-based solder, and the bismuth-based solder comprises one, two or three of BiAg2.5, BiAg10 or BiSb10Ag2.5; The solder with a melting temperature of 280-380° C. is a gold-based solder, and the gold-based solder includes one, two or three of AuSn20, AuGe12 and AuSi2.
6. The composition according to claim 1, characterized in that The solder powder is a 200-mesh sieve powder.
7. The composition according to claim 1, characterized in that The composition also contains 0.1‰wt to 5‰wt of infusible particles with uniform particle size distribution.
8. The composition according to claim 7, characterized in that The particle size of the infusible particles is more than three times the particle size of the solder powder.
9. The composition according to claim 1, characterized in that The composition comprises the following raw material components in percentage by weight: Solder powder: 54wt%~85wt%; Flux: 10wt%~40wt%; Adhesive: 3wt%~7wt%; Non-melting particles: 0.5‰wt~5‰wt.
10. A solder preform, characterized in that: The solder sheet is formed by rolling or extrusion using the preformed solder composition according to any one of claims 1 to 9, and the solder sheet has a regular shape or an irregular shape.
11. A method for preparing the solder sheet according to claim 10, characterized in that: The raw material components in the preformed solder composition are mixed to obtain a mixed material, and the mixed material is rolled or extruded at 60-150° C. to obtain the solder sheet.