A method for manufacturing a thin-walled centrifugal cement rod
Through the manufacturing method of thin-wall centrifugal cement poles, including centrifugal molding, steam heating and external grinding, the problem of shrinkage deformation and insufficient hardness during solidification of cement poles is solved, and the effect of high strength and low cracks is achieved.
Patent Information
- Application Number
- CN202211339752.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-27
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-10-27
AI Technical Summary
The existing cement pole manufacturing methods produce large shrinkage deformation during the solidification of concrete after centrifugation, which is prone to microcracks, affecting the overall strength of thin-walled cement poles, and having poor hardness.
A thin-wall centrifugal cement rod is used to manufacture the cement rod raw materials and match the mold, perform centrifugal molding and perform mixed solution rinsing and sanding treatment, followed by steam heating and cooling, and finally cut and external grinding.
It effectively avoids shrinkage of cement poles, improves overall strength, reduces cracks and seepage, and is simple in production process.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of cement rod processing, in particular to a method for manufacturing a thin-wall centrifugal cement rod. Background Art
[0002] At present, the common manufacturing method of cement poles is mainly made by centrifugal molding process, which is to first load the prepared reinforcement skeleton into the centrifugal mold, then load the mixed concrete into the mold, adjust the mold and place it on the centrifuge, rotate the centrifuge to make the concrete evenly distributed on the inner wall of the mold, and at the same time, the reinforcement skeleton is buried in it. Remove the mold from the centrifuge, wait for the concrete to solidify, steam curing, and then cool and demould to complete the main production process.
[0003] The existing manufacturing process produces large shrinkage deformation during the solidification of concrete after centrifugation, which is prone to produce microcracks, affecting the overall strength of the thin-walled cement rod, and the cement rod produced has poor hardness. To address the above problems, we propose a manufacturing method for thin-walled centrifugal cement rods. Summary of the invention
[0004] 1. Technical issues to be resolved
[0005] In view of the shortcomings of the prior art, the present invention provides a method for manufacturing thin-walled centrifugal cement rods, which solves the problems that the existing manufacturing process produces large shrinkage deformation during the solidification of concrete after centrifugation, easily generates microcracks, affects the overall strength of the thin-walled cement rods, and the hardness of the manufactured cement rods is poor.
[0006] (II) Technical solution
[0007] To achieve the above objectives, the present invention is implemented through the following technical solutions: a method for manufacturing a thin-walled centrifugal cement rod, comprising the following manufacturing method:
[0008] S1, making raw materials for cement poles and making molds matching the cement poles;
[0009] S2, pouring cement rod raw materials into a mold, and sending the mold to a centrifuge for rotation to form a wet blank;
[0010] S3, solidifying and molding the wet blank, demolding it, washing its exterior with the mixed solution, and sanding the hollow interior thereof;
[0011] S4, heat treating the formed cement pole by steam heating, and cooling after completion;
[0012] S5, cut the completed cement pole and polish the outside evenly.
[0013] As a further preferred embodiment of the present invention, in step S1, cement is made, and a quartz mixed raw material is selected: the raw material includes 3-7 parts of silica fume powder, 2-4 parts of zeolite powder, 2-4 parts of bentonite, 10-14 parts of talc, 10-14 parts of calcium stearate, 5-9 parts of coal gangue desulfurization gypsum, 10-24 parts of limestone, 10-14 parts of gypsum, 10-15 parts of iron ore powder, 3-8 parts of clay, and 2-8 parts of modifier. The raw material is first ground, and the granular material is added with pure water and a water reducer and put into a ball mill for wet grinding for 4-8 hours before discharging, and the raw materials are heated, mixed and fully stirred.
[0014] As a further preferred embodiment of the present invention, in step S2, the mold can be preheated in advance by inputting steam for preheating, and the temperature of the input steam is 101°C-111°C. The processed raw cement can also be preheated, and the processing temperature is 63°C-72°C.
[0015] As a further preferred embodiment of the present invention, in step S2, the hollow part during the centrifugal rotation process can be processed, the numerical simulation model of the aperture of the cement rod can be pre-calculated, and the core defect area can be determined, and a guide rod or a guide plate can be inserted into the center of the core defect area to perform raw material removal in conjunction with the effect of centrifugal rotation, and the diameter range value of the flow area of the core defect area can be recorded. The guide rod can scrape out excess material of the aperture until a value equal to the pre-set value is produced.
[0016] As a further preferred embodiment of the present invention, in step S3, the components of the mixed solution are 8-15 parts of magnesium oxide, 6-18 parts of magnesium chloride, 0.5-4 parts of calcium hydroxide, 0.3-1.5 parts of calcium carbonate, 0.3-1.5 parts of ferrous sulfate, 0.3-1 parts of aluminum chloride, 0.3-1.5 parts of calcium nitrate, 4-6 parts of calcium hydroxide, and 2-8 parts of calcium chloride.
[0017] As a further preferred embodiment of the present invention, the steam heating in step S4 can continuously inject pure water with a concentration of 24%-32%. After adding the pure water, calcium bicarbonate water with a concentration of 78% is added. During the heating process, the cement rod is rotated at a speed of 6 rpm for 1.5 hours, and then the rotation speed is changed to 8 rpm-24 rpm to maintain uniform and continuous acceleration.
[0018] As a further preferred embodiment of the present invention, in step S5, the cut cement rods are sent to a steam heating tank for heating; then sent to an auxiliary heating furnace, maintained at 110-135°C, then taken out and allowed to remain in the air, and the above cooling and stay processes are repeated multiple times.
[0019] (III) Beneficial effects
[0020] The present invention provides a method for manufacturing a thin-walled centrifugal cement rod, which has the following beneficial effects:
[0021] The present invention avoids the shrinkage of cement poles, and the manufactured cement poles are not easy to break, have high overall strength, are not easy to have seepage holes on the outside, have fewer overall cracks, and have a simple manufacturing process. DETAILED DESCRIPTION
[0022] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] The present invention provides a technical solution: a method for manufacturing a thin-walled centrifugal cement rod, comprising the following manufacturing method:
[0024] S1, making raw materials for cement poles and making molds matching the cement poles;
[0025] S2, pouring cement rod raw materials into a mold, and sending the mold to a centrifuge for rotation to form a wet blank;
[0026] S3, solidifying and molding the wet blank, demolding it, washing its exterior with the mixed solution, and sanding the hollow interior thereof;
[0027] S4, heat treating the formed cement pole by steam heating, and cooling after completion;
[0028] S5, cut the completed cement pole and polish the outside evenly.
[0029] In step S1, cement is made, and a quartz mixed raw material is selected: the raw material includes 3-7 parts of silica fume powder, 2-4 parts of zeolite powder, 2-4 parts of bentonite, 10-14 parts of talc, 10-14 parts of calcium stearate, 5-9 parts of coal gangue desulfurization gypsum, 10-24 parts of limestone, 10-14 parts of gypsum, 10-15 parts of iron ore powder, 3-8 parts of clay, and 2-8 parts of modifier. The raw material is first ground, and the granular material is added with pure water and a water reducer and put into a ball mill for wet grinding for 4-8 hours before discharging, and the raw materials are heated, mixed, and fully stirred.
[0030] In step S2, the mold can be preheated in advance by inputting steam for preheating, and the temperature of the input steam is 101°C-111°C. The processed raw cement can also be preheated, and the processing temperature is 63°C-72°C.
[0031] In step S2, the hollow part during the centrifugal rotation process can be processed, the numerical simulation model of the aperture of the cement rod is pre-calculated, and the core defect area is determined, and a guide rod or a guide plate is inserted into the center of the core defect area to cut the raw material in accordance with the effect of centrifugal rotation, and the diameter range value of the flow area of the core defect area is recorded. The guide rod scrapes out the excess material of the aperture until the aperture is equal to the pre-set value.
[0032] Step S3, the components of the mixed solution are 8-15 parts of magnesium oxide, 6-18 parts of magnesium chloride, 0.5-4 parts of calcium hydroxide, 0.3-1.5 parts of calcium carbonate, 0.3-1.5 parts of ferrous sulfate, 0.3-1 parts of aluminum chloride, 0.3-1.5 parts of calcium nitrate, 4-6 parts of calcium hydroxide, and 2-8 parts of calcium chloride.
[0033] In step S4, steam heating is performed by continuously injecting pure water with a concentration of 24%-32%. After adding the pure water, calcium bicarbonate water with a concentration of 78% is added. During the heating process, the cement rod is rotated at a speed of 6 rpm for 1.5 hours, and then the rotation speed is changed to 8 rpm-24 rpm, maintaining uniform and continuous acceleration.
[0034] In step S5, the cut cement rods are sent to a steam heating tank for heating; then sent to an auxiliary heating furnace, maintained at 110-135°C, and then taken out and left in the air, and the above cooling and staying process is repeated multiple times.
[0035] Embodiment 1
[0036] A method for manufacturing a thin-walled centrifugal cement rod, wherein the cement is prepared by selecting a quartz mixed raw material: the raw material comprises 7 parts of silica fume powder, 4 parts of zeolite powder, 4 parts of bentonite, 14 parts of talcum powder, 14 parts of calcium stearate, 9 parts of coal gangue desulfurization gypsum, 24 parts of limestone, 14 parts of gypsum, 15 parts of iron ore powder, 8 parts of clay, and 8 parts of a modifier. The raw material is first ground, and the granular material is added with pure water and a water reducing agent and put into a ball mill for wet grinding for 8 hours before discharging the material. The raw material is heated, mixed, and fully stirred, and a mold matching the cement rod is prepared. The mold can be pre-prepared. Heat treatment, using input steam preheating, the temperature of the input steam is 111 ° C, the processed raw cement can also be preheated, the treatment temperature is 72 ° C; the cement rod raw material is poured into the mold, the mold is sent to the centrifuge for rotation to form a wet blank, the hollow part during the centrifugal rotation process can be processed, the aperture numerical simulation model of the cement rod is pre-calculated, and the core defect area is determined, and a guide rod or guide piece is inserted into the center of the core defect area, and the raw material is cut in coordination with the effect of centrifugal rotation, and the diameter of the flow area of the core defect area is recorded The guide rod scrapes out the excess material of the aperture until it is equal to the preset value; the wet blank is solidified and formed, then demolded, and its exterior is rinsed with a mixed solution, the composition ratio of the mixed solution is 15 parts of magnesium oxide, 18 parts of magnesium chloride, 4 parts of calcium hydroxide, 1.5 parts of calcium carbonate, 1.5 parts of ferrous sulfate, 1 part of aluminum chloride, 1.5 parts of calcium nitrate, 6 parts of calcium hydroxide, 8 parts of calcium chloride, and then the internal hollow position is sanded; the formed cement rod is heat treated by steam heating, steam heating, and continuous injection of concentrated The concentration is 32% pure water. After adding pure water, add 78% calcium bicarbonate water. During the heating process, keep rotating the cement rod at a speed of 6rpm for 1.5h, then change the rotation speed to 24rpm, keep accelerating evenly, and cool after completion; cut the completed cement rod, send the cut cement rod into a steam heating tank for heating; then send it into an auxiliary heating furnace, keep it at 135℃, then take it out and let it stay in the air, repeat the above cooling and staying process many times, and complete the uniform grinding of the outside.
[0037] Embodiment 2
[0038] A method for manufacturing a thin-walled centrifugal cement rod, wherein the cement is prepared by selecting a quartz mixed raw material: the quartz mixed raw material includes 3 parts of silica fume powder, 2 parts of zeolite powder, 2 parts of bentonite, 10 parts of talcum powder, 10 parts of calcium stearate, 5 parts of coal gangue desulfurization gypsum, 10 parts of limestone, 10-14 parts of gypsum, 10 parts of iron ore powder, 3 parts of clay, and 2 parts of a modifier. The raw material is first ground, and the granular material is added with pure water and a water reducing agent and put into a ball mill for wet grinding for 8 hours before discharging the material. The raw material is heated, mixed, and fully stirred, and a mold matching the cement rod is manufactured. The mold can be preheated in advance by inputting steam for preheating, and the temperature of the input steam is 111°C. The processed raw cement can also be preheated at a processing temperature of 63°C; the cement rod raw material is poured into the mold, and the mold is sent to the centrifuge for rotation to form a wet blank. The hollow part during the centrifugal rotation process can be processed, the aperture numerical simulation model of the cement rod is calculated in advance, and the core defect area is determined, and a guide rod or a guide piece is inserted into the central part of the core defect area, and the raw material is cut in coordination with the effect of centrifugal rotation, and the core defect area is recorded. The diameter range value of the flow area is set, and the guide rod scrapes out the excess material of the aperture until it is equal to the preset value; the wet blank is solidified and formed, then demolded, and its exterior is rinsed with a mixed solution. The composition ratio of the mixed solution is 8 parts of magnesium oxide, 6 parts of magnesium chloride, 0.5 parts of calcium hydroxide, 0.3 parts of calcium carbonate, 0.3 parts of ferrous sulfate, 0.3 parts of aluminum chloride, 0.3 parts of calcium nitrate, 4 parts of calcium hydroxide, and 2 parts of calcium chloride. The internal hollow position is then sanded; the formed cement rod is heat treated by steam heating. Steam heating, Continuously inject pure water with a concentration of 24%, and then add calcium bicarbonate water with a concentration of 78%. During the heating process, keep rotating the cement rod at a speed of 6rpm for 1.5h, then change the rotation speed to 8rpm, maintain uniform and continuous acceleration, and cool after completion; cut the completed cement rod, send the cut cement rod into a steam heating tank for heating; then send it into an auxiliary heating furnace, maintain 110℃, then take it out and stay in the air, repeat the above cooling and staying process many times, and complete the uniform external grinding.
[0039] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It is obvious to those skilled in the art that the present invention is not limited to the details of the above exemplary embodiments, and the present invention can be implemented in other specific forms without departing from the spirit or basic features of the present invention. Therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive. The scope of the present invention is defined by the attached claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims are included in the present invention. Any mark in the claims should not be regarded as limiting the claims involved.
[0040] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A method for manufacturing a thin-walled centrifugal cement rod, It is characterized in that Including the following production methods, S1, making raw materials for cement poles and making molds matching the cement poles; S2, pouring cement rod raw materials into a mold, and sending the mold to a centrifuge for rotation to form a wet blank; S3, solidifying and molding the wet blank, demolding it, washing its exterior with the mixed solution, and sanding the hollow interior thereof; S4, heat treating the formed cement pole by steam heating, and cooling after completion; S5, cutting the completed cement pole and polishing the outside evenly; To make cement, a quartz mixed raw material is selected: the raw material includes 3-7 parts of silica fume, 2-4 parts of zeolite powder, 2-4 parts of bentonite, 10-14 parts of talc, 10-14 parts of calcium stearate, 5-9 parts of coal gangue desulfurization gypsum, 10-24 parts of limestone, 10-14 parts of gypsum, 10-15 parts of iron ore powder, 3-8 parts of clay, and 2-8 parts of modifier. The raw material is first ground, and the granular material is added with pure water and a water reducing agent and put into a ball mill for wet grinding for 4-8 hours before discharging, and the raw materials are heated, mixed, and fully stirred; The ingredients of the mixed solution are 8-15 parts of magnesium oxide, 6-18 parts of magnesium chloride, 0.5-4 parts of calcium hydroxide, 0.3-1.5 parts of calcium carbonate, 0.3-1.5 parts of ferrous sulfate, 0.3-1 parts of aluminum chloride, 0.3-1.5 parts of calcium nitrate, 4-6 parts of calcium hydroxide, and 2-8 parts of calcium chloride.
2. A method for manufacturing a thin-walled centrifugal cement rod according to claim 1, It is characterized in that In step S2, the mold is preheated in advance by inputting steam for preheating, the temperature of the input steam is 101°C-111°C, and the processed raw cement is preheated at a processing temperature of 63°C-72°C.
3. The method for manufacturing a thin-walled centrifugal cement rod according to claim 1, It is characterized in that In step S2, the hollow part during the centrifugal rotation process is processed, the numerical simulation model of the aperture of the cement rod is calculated in advance, and the core defect area is determined, and a guide rod or a guide plate is inserted into the center of the core defect area to cut the raw material in coordination with the effect of centrifugal rotation, and the diameter range value of the flow area of the core defect area is recorded. The guide rod scrapes out the excess material of the aperture until the aperture is equal to the pre-set value.
4. A method for manufacturing a thin-walled centrifugal cement rod according to claim 1, It is characterized in that In step S5, the cut cement rods are sent to a steam heating tank for heating; then sent to an auxiliary heating furnace, maintained at 110-135°C, and then taken out and left in the air, and the above cooling and staying process is repeated multiple times.
Citation Information
Patent Citations
Preparation method of anti-cracking autoclaved brick
CN107512874A
Method for processing cement pipe piles by carbon fibers and recycled concrete
CN109400029A
Tubular pile steam treatment method
CN112318703A
Method for softening water for boiler steam
CN112979032A
Preparation method and system for partial prestressed concrete pile foundation for power transmission line tower
CN113119296A