An environmentally friendly water-based digital printing film
By using a combined structure of breathable coating, base paper layer, release layer and ink-absorbing layer in the digital printing film, the problem of thermal deformation and air impermeability of the PET film is solved, and the high efficiency of the environmentally friendly water-based digital printing film is achieved. printing and low-carbon environmental goals.
Patent Information
- Application Number
- CN202310090402.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-09
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-02-09
AI Technical Summary
Traditional latex ink digital printing film materials are based on PET film materials, which have problems of thermal deformation, air tightness and environmental pollution. In addition, paper-based materials easily absorb water during the printing process, causing wet deformation, which affects printing quality and equipment operation.
It uses an environmentally friendly water-based digital printing film material composed of a breathable coating, a base paper layer, a release layer, an ink-absorbing layer and a water-absorbing layer. The breathable coating is made of kaolin, diatomaceous earth, polyvinyl alcohol and other materials. Polystyrene , PET and other materials are made of release layer, defoaming agent, silica aerogel and other materials are made of ink-absorbing layer, cross-linked carboxymethylcellulose grafted with acrylamide and other materials are made of water-absorbing layer, combined with micro-heat curing and cutting process to form a suitable printing film structure.
It effectively avoids paper wet deformation, improves substrate transparency and printing quality, reduces wet deformation and environmental pollution, and meets low-carbon and environmentally friendly application requirements.
Smart Images

Figure CN115848048B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of printing film materials, and in particular relates to an environmentally friendly water-based digital printing film material. Background Art
[0002] Latex ink is an ink that can be printed on uncoated media. Based on the pigment base material and resin and latex additive formula of pigment ink, latex ink has the advantages of adapting to the diversity of printing media and imaging persistence of previous solvent-based inks, while also having the durability and environmental protection of water-based inks for equipment. It is a functional ink that represents the future direction of inkjet printing. Latex ink can be printed on uncoated media. It has the advantages of adapting to the diversity of printing media and imaging persistence of previous solvent-based inks, while also having the durability and environmental protection of water-based inks for equipment. This determines that this ink has a very wide range of applications. It can be used to produce and print various types of advertising graphics, home decoration, wallpaper, transparent gauze, photo studios, canvas, non-woven fabrics, leather printing and other coated and uncoated materials.
[0003] The patent specification with the publication number CN113263850B provides a latex ink digital printing film material and a preparation method thereof for improving the phenomenon of fading after washing. The printing film material includes a carrier base, a silicone protective coating, a thermal peeling coating and a latex ink absorbing medium coating from bottom to top; the preparation method of the printing film material includes: surface treatment of the carrier base, coating the surface of the carrier base with a silicone protective coating, coating the surface of the silicone protective coating with a thermal peeling coating, coating the surface of the thermal peeling coating with a latex ink absorbing medium coating, and cutting according to the required size after the above layers are completely dried. By designing the silicone protective coating, the thermal peeling coating and the latex ink absorbing medium coating, the phenomenon of fading after washing can be effectively improved. At the same time, the latex ink digital printing film material is suitable for a digital offset heat transfer system and has the advantage of low-cost application.
[0004] However, the above-mentioned latex ink digital printing film is based on PET film, and during the roll-to-roll thermal transfer process, the PET film is deformed by heat, causing the pattern transfer to deform and cannot be transferred in large quantities; because the PET film is not breathable and is completely closed, the pattern layer after transfer is also a closed system, and a breathable layer cannot be formed on the surface of the fabric, affecting the wearing and feel; the thermal transfer after transfer needs to be recycled, which is easy to cause secondary environmental pollution. Using paper substrates can effectively solve the above problems, resist thermal deformation, solve the problem of breathability, and waste paper can be recycled, but paper-based materials have large wet deformation after absorbing water during the printing process, which makes the paper easily warp, affecting the operation of the printer; the paper is opaque, and the quality of the printed pattern cannot be observed, affecting the inspection of semi-finished products, etc.
[0005] In view of this, it is necessary to provide an environmentally friendly water-based digital printing film material and a preparation method thereof, which can replace paper-based functional materials and conform to the global trend of low-carbon environmental protection and replacing plastic with paper. Summary of the invention
[0006] The purpose of the present invention is to overcome the above problems existing in the conventional technology and to provide an environmentally friendly water-based digital printing film material and a preparation method thereof.
[0007] In order to achieve the above technical objectives and the above technical effects, the present invention is implemented through the following technical solutions:
[0008] An environmentally friendly water-based digital printing film material comprises, from bottom to top, a breathable coating layer, a base paper layer, a release layer, an ink absorbing layer and a water absorbing layer.
[0009] Furthermore, in the above-mentioned environmentally friendly water-based digital printing film material, the material of the base paper layer is a base paper material with a wet change of less than 3%.
[0010] Furthermore, in the above-mentioned environmentally friendly water-based digital printing film material, the breathable coating is made by mixing the following components in proportion:
[0011] Kaolin 15-35%,
[0012] Diatomaceous earth 20-40%,
[0013] The balance is polyvinyl alcohol, and the sum of the weight percentages of each component is 100%;
[0014] The preparation method of the breathable coating is as follows: weigh the components in proportion, ball-mill kaolin and diatomaceous earth, add them into polyvinyl alcohol, and stir to mix well.
[0015] Furthermore, in the above-mentioned environmentally friendly water-based digital printing film material, the release layer is made by mixing the following components in proportion:
[0016] Polystyrene 40-60%,
[0017] PET 20-27%,
[0018] PTA 10-17%,
[0019] Beeswax 8-12%,
[0020] Antioxidants 1-2%,
[0021] Defoamer 1-2%,
[0022] The sum of the weight percentages of the above components is 100%;
[0023] The preparation method of the release layer is as follows: weigh the components in proportion, heat the polystyrene, PET, PTA and beeswax into fluids, and then stir and mix them together with the antioxidant and the defoaming agent.
[0024] Furthermore, in the above-mentioned environmentally friendly water-based digital printing film material, the ink-absorbing layer is made by mixing the following components in proportion:
[0025] Defoamer 8-10%,
[0026] Silica aerogel 5-10%,
[0027] Diatomaceous earth 4-6%,
[0028] Titanium dioxide 5-10%,
[0029] The balance is deionized water, and the sum of the weight percentages of the above components is 100%;
[0030] The preparation method of the ink-absorbing layer is as follows: weigh each component in proportion, add titanium dioxide into deionized water and stir at 30-40° C., add silicon dioxide aerogel and diatomaceous earth into defoamer and stir, and then stir and mix the two together.
[0031] Furthermore, in the above-mentioned environmentally friendly water-based digital printing film material, the water-absorbing layer is made by mixing the following components in proportion:
[0032] Cross-linked carboxymethyl cellulose grafted with acrylamide 20-35%,
[0033] Isopropyl alcohol 30-50%,
[0034] Ethylenediamine curing agent 3-6%,
[0035] Alkylphenol polyoxyethylene ether penetrant 2-4%,
[0036] The balance is ethylene-acrylic acid copolymer, and the sum of the weight percentages of the above components is 100%;
[0037] The preparation method of the water absorbing layer is: weigh each component according to proportion, and stir and mix them together.
[0038] Furthermore, the preparation method of the environmentally friendly water-based digital printing film material as described above comprises the following steps:
[0039] 1) Surface treatment of the base paper layer to control its peel strength to 280-400 g / inch;
[0040] 2) Applying the breathable coating: evenly apply the composition liquid of the breathable coating on the back of the treated base paper layer, and slightly heat cure to obtain the breathable coating;
[0041] 3) Coating of release layer: uniformly coating the composition liquid of the release layer on the front side of the base paper layer, and slightly curing the release layer by heat treatment to obtain the release layer;
[0042] 4) Coating of ink absorbing layer: coating the composition liquid of the ink absorbing layer on the release layer, and slightly curing it with heat to obtain the ink absorbing layer;
[0043] 5) coating of the water absorbing layer: coating the composition liquid of the water absorbing layer on the ink absorbing layer, and curing with slight heat to obtain the water absorbing layer;
[0044] 6) Cutting: After the above layers are completely dry, cut according to the required size.
[0045] Furthermore, the application method of the environmentally friendly water-based digital printing film material as described above comprises the following steps:
[0046] 1) Printing pattern film;
[0047] 2) Sprinkle the polyurethane hot melt adhesive white powder on the printing film after inkjet printing, and transfer the hot melt adhesive powder on the surface of the pattern as a transfer adhesive layer medium to the object to be printed, so as to bond the pattern and the object to be printed;
[0048] 3) After the bright film is printed, the coating is completely cooled and brittle, and the base paper layer is peeled off.
[0049] The beneficial effects of the present invention are:
[0050] 1. In order to solve the problem of paper deformation during wet processing, the paper base material with a wet deformation of less than 3% should be selected to effectively avoid the warping of the printing medium.
[0051] 2. The present invention applies a breathable coating on the back of the base paper layer, which can improve the transparency of the substrate and basically solve the problem of pattern quality inspection; the breathable coating is a porous film-forming structure with polyvinyl alcohol + kaolin + diatomaceous earth as main materials, which is not affected by large ink printing. Polyvinyl alcohol is used as a water-based resin to achieve film-forming and water-isolating effects. Kaolin uses high porosity to achieve water absorption, thereby reducing the wet change of the base paper layer. The porosity, incompressibility and chemical stability of diatomaceous earth make its surface have good adsorption properties.
[0052] Of course, any product implementing the present invention does not necessarily need to achieve all of the above advantages at the same time. BRIEF DESCRIPTION OF THE DRAWINGS
[0053] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.
[0054] Figure 1 It is a schematic diagram of the composition of the printing film material in the present invention;
[0055] Figure 2 It is a schematic diagram of the structure of the breathable coating in the present invention;
[0056] 1- breathable coating, 2- base paper layer, 3- release layer, 4- ink absorbing layer, 5- water absorbing layer. DETAILED DESCRIPTION
[0057] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0058] An environmentally friendly water-based digital printing film material, such as Figure 1-Figure 2 As shown, the printing film material includes a breathable coating layer 1, a base paper layer 2, a release layer 3, an ink absorbing layer 4 and a water absorbing layer 5 from bottom to top.
[0059] The base paper layer is made of base paper material with a wet change of less than 3%.
[0060] The breathable coating is made by mixing the following components in proportion:
[0061] Kaolin 15-35%,
[0062] Diatomaceous earth 20-40%,
[0063] The balance is polyvinyl alcohol, and the sum of the weight percentages of each component is 100%;
[0064] The preparation method of the breathable coating is as follows: weigh the components in proportion, ball-mill kaolin and diatomaceous earth, add them into polyvinyl alcohol, and stir to mix well.
[0065] Wherein, the release layer is made by mixing the following components in proportion:
[0066] Polystyrene 40-60%,
[0067] PET 20-27%,
[0068] PTA 10-17%,
[0069] Beeswax 8-12%,
[0070] Antioxidants 1-2%,
[0071] Defoamer 1-2%,
[0072] The sum of the weight percentages of the above components is 100%;
[0073] The preparation method of the release layer is as follows: weigh the components in proportion, heat the polystyrene, PET, PTA and beeswax into fluids, and then stir and mix them together with the antioxidant and the defoaming agent.
[0074] Wherein, the ink absorbing layer is made by mixing the following components in proportion:
[0075] Defoamer 8-10%,
[0076] Silica aerogel 5-10%,
[0077] Diatomaceous earth 4-6%,
[0078] Titanium dioxide 5-10%,
[0079] The balance is deionized water, and the sum of the weight percentages of the above components is 100%;
[0080] The preparation method of the ink-absorbing layer is as follows: weigh each component in proportion, add titanium dioxide into deionized water and stir at 30-40° C., add silicon dioxide aerogel and diatomaceous earth into defoamer and stir, and then stir and mix the two together.
[0081] Wherein, the water absorbing layer is prepared by mixing the following components in proportion:
[0082] Cross-linked carboxymethyl cellulose grafted with acrylamide 20-35%,
[0083] Isopropyl alcohol 30-50%,
[0084] Ethylenediamine curing agent 3-6%,
[0085] Alkylphenol polyoxyethylene ether penetrant 2-4%,
[0086] The balance is ethylene-acrylic acid copolymer, and the sum of the weight percentages of the above components is 100%;
[0087] The preparation method of the water absorbing layer is: weigh each component according to proportion, and stir and mix them together.
[0088] An environmentally friendly water-based digital printing film material, the preparation method of which comprises the following steps:
[0089] 1) Surface treatment of the base paper layer to control its peel strength to 280-400 g / inch;
[0090] 2) Applying the breathable coating: evenly apply the composition liquid of the breathable coating on the back of the treated base paper layer, and slightly heat cure to obtain the breathable coating;
[0091] 3) Coating of release layer: uniformly coating the composition liquid of the release layer on the front side of the base paper layer, and slightly curing the release layer by heat treatment to obtain the release layer;
[0092] 4) Coating of ink absorbing layer: coating the composition liquid of the ink absorbing layer on the release layer, and slightly curing it with heat to obtain the ink absorbing layer;
[0093] 5) coating of the water absorbing layer: coating the composition liquid of the water absorbing layer on the ink absorbing layer, and curing it with slight heat to obtain the water absorbing layer;
[0094] 6) Cutting: After the above layers are completely dry, cut according to the required size.
[0095] An environmentally friendly water-based digital printing film material, the application method comprises the following steps:
[0096] 1) Printing pattern film;
[0097] 2) Sprinkle the polyurethane hot melt adhesive white powder on the printing film after inkjet printing, and transfer the hot melt adhesive powder on the surface of the pattern as a transfer adhesive layer medium to the object to be printed (such as fabric), so as to bond the pattern and the object to be printed (such as fabric);
[0098] 3) After the bright film is printed, the coating is completely cooled and brittle, and the base paper layer is peeled off.
[0099] Among them, the ink drying temperature is: 30-40℃, the hot melt powder shaking temperature is: 100-140℃. The hot pressing temperature during the transfer process is: 130-180℃, time: 8-15s, pressure: 3-7kg.
[0100] The relevant specific embodiments of the present invention are as follows:
[0101] Example 1
[0102] An environmentally friendly water-based digital printing film material, the printing film material comprises, from bottom to top, a breathable coating layer 1, a base paper layer 2, a release layer 3, an ink absorbing layer 4 and a water absorbing layer 5, and a preparation method thereof comprises the following steps:
[0103] 1) Surface treatment of the base paper layer to control its peel strength to 280-400 g / inch;
[0104] 2) Applying the breathable coating: 15% kaolin, 40% diatomaceous earth and 45% polyvinyl alcohol are prepared into a composition liquid of the breathable coating; the composition liquid of the breathable coating is evenly applied on the back side of the treated base paper layer, and slightly heat cured to obtain the breathable coating;
[0105] 3) Coating of release layer: 40% polystyrene, 27% PET, 17% PTA, 12% beeswax, 2% antioxidant and 2% defoaming agent are prepared into a composition liquid of release layer; the composition liquid of release layer is evenly coated on the front side of base paper layer, and slightly heat cured to obtain release layer;
[0106] 4) Coating of ink-absorbing layer: 10% of defoamer, 6% of silica aerogel, 4% of diatomaceous earth, 10% of titanium dioxide and 70% of deionized water are prepared into a composition liquid of ink-absorbing layer; the composition liquid of ink-absorbing layer is coated on the release layer, and slightly heat-cured to obtain the ink-absorbing layer;
[0107] 5) coating of water-absorbing layer: preparing a composition liquid of water-absorbing layer by cross-linking carboxymethyl cellulose grafted acrylamide 20%, isopropyl alcohol 50%, ethylenediamine curing agent 3%, alkylphenol polyoxyethylene ether penetrant 4%, and ethylene-acrylic acid copolymer 23%; coating the composition liquid of water-absorbing layer on ink-absorbing layer, and curing by slight heat to obtain water-absorbing layer;
[0108] 6) Cutting: After the above layers are completely dry, cut according to the required size.
[0109] Example 2
[0110] An environmentally friendly water-based digital printing film material, the printing film material comprises, from bottom to top, a breathable coating layer 1, a base paper layer 2, a release layer 3, an ink absorbing layer 4 and a water absorbing layer 5, and a preparation method thereof comprises the following steps:
[0111] 1) Surface treatment of the base paper layer to control its peel strength to 280-400 g / inch;
[0112] 2) Applying the breathable coating: 20% kaolin, 30% diatomaceous earth and 50% polyvinyl alcohol are prepared into a composition liquid of the breathable coating; the composition liquid of the breathable coating is evenly applied on the back side of the treated base paper layer, and slightly heat cured to obtain the breathable coating;
[0113] 3) Coating of release layer: 60% polystyrene, 20% PET, 10% PTA, 8% beeswax, 1% antioxidant, and 1% defoaming agent are prepared into a composition liquid of release layer; the composition liquid of release layer is evenly coated on the front side of the base paper layer, and slightly heat cured to obtain the release layer;
[0114] 4) Coating of ink-absorbing layer: 8% of defoamer, 5% of silica aerogel, 6% of diatomaceous earth, 5% of titanium dioxide and 76% of deionized water are prepared into a composition liquid of ink-absorbing layer; the composition liquid of ink-absorbing layer is coated on the release layer, and slightly heat-cured to obtain the ink-absorbing layer;
[0115] 5) coating of water-absorbing layer: preparing a composition liquid of water-absorbing layer by cross-linking carboxymethyl cellulose grafted acrylamide 28%, isopropyl alcohol 40%, ethylenediamine curing agent 5%, alkylphenol polyoxyethylene ether penetrant 3%, and ethylene-acrylic acid copolymer 24%; coating the composition liquid of water-absorbing layer on ink-absorbing layer, and curing by slight heat to obtain water-absorbing layer;
[0116] 6) Cutting: After the above layers are completely dry, cut according to the required size.
[0117] Example 3
[0118] An environmentally friendly water-based digital printing film material, the printing film material comprises, from bottom to top, a breathable coating layer 1, a base paper layer 2, a release layer 3, an ink absorbing layer 4 and a water absorbing layer 5, and a preparation method thereof comprises the following steps:
[0119] 1) Surface treatment of the base paper layer to control its peel strength to 280-400 g / inch;
[0120] 2) Applying the breathable coating: 35% kaolin, 20% diatomaceous earth and 45% polyvinyl alcohol are prepared into a composition liquid of the breathable coating; the composition liquid of the breathable coating is evenly applied on the back side of the treated base paper layer, and slightly heat cured to obtain the breathable coating;
[0121] 3) Coating of release layer: 50% polystyrene, 23% PET, 14% PTA, 10% beeswax, 1% antioxidant, and 2% defoaming agent are prepared into a composition liquid of release layer; the composition liquid of release layer is evenly coated on the front side of the base paper layer, and slightly heat cured to obtain the release layer;
[0122] 4) Coating of ink-absorbing layer: 9% of defoamer, 10% of silica aerogel, 5% of diatomaceous earth, 7% of titanium dioxide and 69% of deionized water are prepared into a composition liquid of ink-absorbing layer; the composition liquid of ink-absorbing layer is coated on the release layer, and slightly heat-cured to obtain the ink-absorbing layer;
[0123] 5) coating of water-absorbing layer: preparing a composition liquid of water-absorbing layer by cross-linking carboxymethyl cellulose grafted acrylamide 35%, isopropyl alcohol 30%, ethylenediamine curing agent 6%, alkylphenol polyoxyethylene ether penetrant 2%, and ethylene-acrylic acid copolymer 27%; coating the composition liquid of water-absorbing layer on ink-absorbing layer, and curing by slight heat to obtain water-absorbing layer;
[0124] 6) Cutting: After the above layers are completely dry, cut according to the required size.
[0125] Example 4
[0126] The composition, construction and material selection ideas of the environmentally friendly water-based digital printing film material in the present invention are as follows:
[0127] The relevant setting parameters for machine printing are shown in Table 1:
[0128] Table 1
[0129] Test model HR-PRO600 Heat Press Machine Nozzle Type Epson I3200 dual head Printing accuracy Two-way / 6pass Front lift plate temperature closure Melting temperature 120℃ ink B / C / M / Y / W Pressing temperature 160℃ Pressing time 15s Test software Maintop 6.1 UV Personalized Edition Test image HR special test chart
[0130] The printing process of environmentally friendly water-based digital printing film (DTF paper-based heat transfer printing film): distinguish the front and back of the heat transfer film → print (color first and then white) → sprinkle hot melt powder → dry (hot melt powder is baked to a molten state, 100-120℃) → press (150-170℃, 8-15s) → peel off the substrate → finished product.
[0131] This process is the current conventional process for heat transfer printing. During actual use, the specific process implementation plan needs to be fine-tuned according to the customer's applicable environment, equipment, substrate fabrics, and related consumables.
[0132] Application performance testing:
[0133] a. Paper wet deformation test: The wet deformation of paper is tested by immersion method, which is to immerse the paper in water at a certain temperature, or immerse it in water and then air dry it to measure the relative change in size;
[0134] b. Ink absorption and adsorption test: Test the maximum ink load that papers with different solid content can carry under the test accuracy. The concentration of color ink is 100%, and the concentration of white ink increases step by step from 100% until the ink flows on the paper;
[0135] c. Drying speed test: using the impression method, the experiment should be carried out at a temperature of 20° (± 2°) C and a relative air humidity of 60-65%. When the paint film does not feel sticky when the finger is pressed on the paper film (without any pressure) or no finger marks are left on its surface, it can be considered to be actually dry.
[0136] d. The transparency and smoothness of paper are mainly observed by naked eyes:
[0137] 1) Transparency: If the color of the printed image can be clearly seen from the back of the print, it is considered fair. If it cannot be clearly seen, it is considered poor. If the 5px line can be clearly seen, it is considered good.
[0138] 2) Flatness: Cut A4-width paper into a 50% constant humidity cabinet, and observe the curling of the paper after 24 hours, and make a judgment based on the actual situation;
[0139] e. Machine passability: judge the machine passability based on the actual printing situation;
[0140] Measure three samples on the front and back sides, and express the results as the arithmetic mean of all measured values, and report the maximum and minimum values, as shown in Table 2:
[0141] Table 2
[0142]
[0143] Select 70g paper as the base paper of DTF heat transfer paper base film;
[0144] The base paper layer was tested by coating with DTF coating, and the results are shown in Table 3:
[0145] Table 3
[0146]
[0147] The number of passes is simply the number of times the printing carriage prints back and forth.
[0148] It can be concluded from Table 3 that if the ink is too wet, the hot melt powder in the subsequent process will easily penetrate the ink absorbing layer to the protective layer, and the surface of the final product will have powder particles that affect the finished product;
[0149] Generally speaking, in the actual printing process, medium feather printing can meet the customer's needs for speed and printing quality;
[0150] The quality of kaolin has a great beneficial effect on the printing of DTF paper-based heat transfer printing film, mainly manifested in: 1) the drying speed of ink; 2) the increase of ink carrying capacity; 3) the improvement of wet deformation (expansion rate) of paper;
[0151] At the same time, the test found that due to the compatibility of the coating ink with the paper, the paper base film is not suitable for opening the platform for heating, so it is very easy to cause the ink to flow when printing some dark blocks. In view of this situation, the inventors coated a release layer, an ink absorbing layer and a water absorbing layer on the basis of this isolation coating, and the ink flow was improved, as shown in Table 4:
[0152] Table 4
[0153]
[0154] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. An environmentally friendly water-based digital printing film material, characterized by: The printing film material comprises, from bottom to top, a breathable coating layer, a base paper layer, a release layer, an ink absorbing layer and a water absorbing layer; The breathable coating is prepared by mixing the following components in proportion: Kaolin 15-35%, Diatomaceous earth 20-40%, The balance is polyvinyl alcohol, and the sum of the weight percentages of each component is 100%; The preparation method of the breathable coating is as follows: weigh the components in proportion, ball-mill kaolin and diatomaceous earth, add them into polyvinyl alcohol, and stir to mix well.
2. The environmentally friendly water-based digital printing film material according to claim 1, characterized in that: The base paper layer is made of base paper material with a wet change of less than 3%.
3. The environmentally friendly water-based digital printing film material according to claim 1, characterized in that: The release layer is made by mixing the following components in proportion: Polystyrene 40-60%, PET 20-27%, PTA 10-17%, Beeswax 8-12%, Antioxidants 1-2%, Defoamer 1-2%, The sum of the weight percentages of the above components is 100%; The preparation method of the release layer is as follows: weigh the components in proportion, heat the polystyrene, PET, PTA and beeswax into fluids, and then stir and mix them together with the antioxidant and the defoaming agent.
4. The environmentally friendly water-based digital printing film material according to claim 1, characterized in that: The ink-absorbing layer is made by mixing the following components in proportion: Defoamer 8-10%, Silica aerogel 5-10%, Diatomaceous earth 4-6%, Titanium dioxide 5-10%, The balance is deionized water, and the sum of the weight percentages of the above components is 100%; The preparation method of the ink-absorbing layer is as follows: weigh each component in proportion, add titanium dioxide into deionized water and stir at 30-40° C., add silicon dioxide aerogel and diatomaceous earth into defoamer and stir, and then stir and mix the two together.
5. The environmentally friendly water-based digital printing film material according to claim 1, characterized in that: The water absorbing layer is made by mixing the following components in proportion: Cross-linked carboxymethyl cellulose grafted with acrylamide 20-35%, Isopropyl alcohol 30-50%, Ethylenediamine curing agent 3-6%, Alkylphenol polyoxyethylene ether penetrant 2-4%, The balance is ethylene-acrylic acid copolymer, and the sum of the weight percentages of the above components is 100%; The preparation method of the water absorbing layer is: weigh each component according to proportion, and stir and mix them together.
6. The environmentally friendly water-based digital printing film material according to any one of claims 1 to 5, characterized in that: The method for preparing the printing film material comprises the following steps: 1) Surface treatment of the base paper layer to control its peel strength to 280-400 g / inch; 2) Applying the breathable coating: evenly apply the composition liquid of the breathable coating on the back of the treated base paper layer, and slightly heat cure to obtain the breathable coating; 3) Coating of release layer: uniformly coating the composition liquid of the release layer on the front side of the base paper layer, and slightly curing the release layer by heat treatment to obtain the release layer; 4) Coating of ink absorbing layer: coating the composition liquid of the ink absorbing layer on the release layer, and slightly curing it with heat to obtain the ink absorbing layer; 5) coating of the water absorbing layer: coating the composition liquid of the water absorbing layer on the ink absorbing layer, and curing with slight heat to obtain the water absorbing layer; 6) Cutting: After the above layers are completely dry, cut according to the required size.
7. The environmentally friendly water-based digital printing film material according to any one of claims 1 to 5, characterized in that: The application method of the printing film material comprises the following steps: 1) Printing pattern film; 2) Sprinkle the polyurethane hot melt adhesive white powder on the printing film after inkjet printing, and transfer the hot melt adhesive powder on the surface of the pattern as a transfer adhesive layer medium to the object to be printed, so as to bond the pattern and the object to be printed; 3) After the bright film is printed, the coating is completely cooled and brittle, and the base paper layer is peeled off.
Citation Information
Patent Citations
A latex ink digital printing film material with improved water washing fading phenomenon and its preparation method
CN113263850B
Tacky microporous transfer material
CN109153276A
Latex ink digital printing film material for improving washing fading phenomenon and preparation method thereof
CN113263850A
Thermal transfer printing decal paper for automatic decal machine and preparation method of thermal transfer printing decal paper
CN113954562A
Ink-jet recording image offset medium and image offset method thereof
CN1200992A