A new backfill material suitable for assembled shaft support and its preparation method and application
By adjusting the proportion of two-component foam materials, a filling material with high early strength and good toughness is prepared and filled behind the corrugated plate, which solves the problem of stress concentration in the construction of prefabricated shafts and improves the stability and safety of the supporting structure. , achieving low-cost and efficient construction results.
Patent Information
- Application Number
- CN202211482651.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-24
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-11-24
AI Technical Summary
During the construction of prefabricated shafts, the contact between corrugated plates and surrounding rock or concrete primary support structures can easily cause stress concentration, leading to structural damage and safety hazards. There is a lack of a filling material with high early strength and excellent mechanical properties to improve the stability of the supporting structure. sex.
Using two-component foaming materials of component A and component B, by adjusting diphenylmethane diisocyanate, polymethylene polyphenyl isocyanate, polyether tetraol, polyether triol, catalyst, and chain extension crosslinking By adjusting the ratio of joint agent, foam stabilizer, plasticizer and foaming agent, a filling material with high early strength, good toughness, corrosion resistance and water resistance is prepared and filled behind the corrugated board to increase the bonding strength and optimize stress distribution.
It effectively increases the contact area between the corrugated plate and the surrounding rock or concrete, enhances the bonding strength, improves construction safety, and achieves low-cost, low-energy mass production through a simple and efficient process.
Smart Images

Figure BDA0003962355570000121
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of backfill materials, and in particular relates to a new backfill material suitable for assembled shaft support, a preparation method and an application thereof. Background Art
[0002] A vertical shaft is a well-shaped pipe with an upright cave wall, which is square, long or irregularly circular in plan. Since vertical shaft construction has the advantages of small footprint and less interference with surrounding construction, it is widely used in water intake, water diversion, ventilation, slag removal, and air replenishment in water conservancy and hydropower projects. However, the construction space in the vertical shaft is small, the construction period is long, there are many high-altitude and edge operations, and it is inconvenient to pass. Therefore, during the construction of the vertical shaft, a support structure is needed to fix and support the construction personnel and related equipment through the support structure to complete the construction.
[0003] In the process of prefabricated shaft construction, corrugated plates are often used as supporting structures. As a steel material, corrugated plates have the advantages of strong mechanical properties, anti-aging, and easy installation. However, due to its corrugated structure, it is in linear contact with the surrounding rock or concrete primary support structure behind it, which is prone to stress concentration. In addition, the underground stress field is complex, and sudden loads will cause structural damage, endangering the safety of the shaft.
[0004] In summary, how to develop a filling material with good bonding ability with corrugated plates, high early strength and excellent mechanical properties in view of the particularity of prefabricated shaft construction is a technical problem that needs to be solved urgently by technical personnel in this field. A new material with simple process, short curing time, high early strength, good mechanical properties, corrosion resistance and good waterproofness is a problem that needs to be solved urgently by technical personnel in this field. Summary of the invention
[0005] The purpose of the present invention is to provide a new backfill material suitable for assembled shaft support, through the selection of raw materials of component A and component B and the adjustment of dosage, a filling material with high early strength, good toughness, strong mechanical properties, corrosion resistance and good waterproofness is obtained. Filling it behind the corrugated plate can effectively increase the contact area between the support structure and the surrounding rock or concrete primary support, increase the bonding strength, and improve the safety of production operations.
[0006] To achieve the above object, the present invention provides a new backfill material suitable for assembled shaft support, which comprises component A and component B by weight, wherein:
[0007] Component A includes:
[0008] 10-30 parts of diphenylmethane diisocyanate;
[0009] 70-90 parts of polymethylene polyphenyl isocyanate;
[0010] Component B includes:
[0011] 40-60 parts of polyether tetraol;
[0012] 35-55 parts of polyether triol;
[0013] 1.8-2.2 parts of catalyst;
[0014] 1.8 to 2.2 parts of chain extension crosslinking agent;
[0015] 2 to 4 parts of foam stabilizer;
[0016] 10-30 parts of plasticizer;
[0017] 5 to 10 parts of foaming agent.
[0018] In a preferred embodiment, the weight ratio of component A to component B is 1:1.
[0019] In a preferred embodiment, the molecular weight of the polyether tetraol in component B is 500, and the molecular weight of the polyether triol is 550.
[0020] In a preferred embodiment, the polyether tetraol in component B is polyether 4110G, and the polyether triol is polyether GP-305.
[0021] In a preferred embodiment, the catalyst includes one or two of dibutyltin dilaurate and 33% concentration of triethylenediamine;
[0022] The chain extending cross-linking agent is 1,4-butanediol;
[0023] The foam stabilizer is an organosilicon copolymer;
[0024] The plasticizer is dioctyl phthalate;
[0025] The foaming agent is one or two of distilled water and monofluorodichloroethane.
[0026] In a preferred embodiment, the catalyst is composed of dibutyltin dilaurate and 33% concentration of triethylenediamine in a mass ratio of 1: (0.4-0.55);
[0027] The foaming agent is composed of distilled water and monofluorodichloroethane in a mass ratio of 1: (5-6).
[0028] Another object of the present invention is to provide a method for preparing a new backfill material suitable for assembled shaft support, which can be prepared by mixing component A and component B separately. The overall process is simple and efficient, and the mixing can be completed at room temperature. The equipment and energy consumption requirements are low, and the preparation process is highly safe, which is particularly suitable for large-scale industrial production. The prepared component A and component B have good stability, are easy to store and transport, and can be sold separately as commercial products.
[0029] To achieve the above object, the present invention provides a method for preparing a new backfill material suitable for assembled shaft support, which specifically comprises the following steps:
[0030] Preparation of component A: Weigh diphenylmethane diisocyanate and polymethylene polyphenyl isocyanate in parts by weight, and mix them evenly at room temperature to obtain component A;
[0031] Preparation of component B:
[0032] (1) Weighing the polyether tetraol and polyether triol in component B by weight, mixing at room temperature, and drying to obtain a mixed polyether polyol;
[0033] (2) Add a catalyst, a chain extender, a cross-linking agent, a foam stabilizer, a foaming agent and a plasticizer to the mixed polyether polyol, and stir evenly at room temperature to obtain the obtained product.
[0034] In a preferred embodiment, in step (1), the drying treatment conditions are: drying at 40-60° C. for 12-24 hours.
[0035] Another object of the present invention is to provide an application method of a new type of back-filling material suitable for prefabricated shaft support. When filling the back of the corrugated plate of the prefabricated shaft support, the material is injected into the space between the corrugated plate and the surrounding rock in a liquid state, foams and expands, and is filled into each gap under the push of the expansion force, forming a buffer zone between the corrugated plate and the surrounding rock, changing the line contact between the two in the prior art into surface contact, releasing stress through deformation, thereby increasing the force-bearing area, optimizing stress distribution, and improving the stability of the support structure.
[0036] To achieve the above object, the present invention provides an application method of a new backfill material suitable for assembled shaft support, which specifically comprises the following steps:
[0037] At the construction site, component A and component B are respectively poured into a two-component foaming machine, and a mixed slurry is obtained through the foaming reaction. The mixed slurry is injected into the space between the shaft and the supporting structure through the grouting holes to foam and generate the filling material behind the shaft support.
[0038] In a preferred embodiment, the new backfill material suitable for prefabricated shaft support has an underground depth of up to 475m, a ground stress of up to 14.46MPa, a foaming temperature of 30-80°C, and the outer filling material includes one or more of metal, concrete, and rock.
[0039] Compared with the prior art, the technical solution of the present invention has the following advantages:
[0040] The present invention uses low-cost, easy-to-procure raw materials, and a one-step synthesis process that is simple, efficient, and low-energy to synthesize a corrugated plate backfill material with high early strength, good toughness, low expansion force, and high foaming rate. When injected between the assembled shaft corrugated plate and the surrounding rock, it can quickly foam and expand, and further fill into each gap under the impetus of the expansion force, forming a buffer zone between the corrugated plate and the surrounding rock, releasing stress through deformation, optimizing stress distribution, and thus improving the connection effect between the corrugated plate and the surrounding rock. DETAILED DESCRIPTION
[0041] In order to enable those skilled in the art to better understand the present invention, the present invention is further described in detail below by means of specific implementation modes, but it should be understood that the protection scope of the present invention is not limited by the specific implementation modes.
[0042] The embodiments of the present invention solve the problems of stress concentration and poor stability in the prior art between the steel corrugated plate and the surrounding rock or concrete primary support structure behind it by providing a new back-filling material suitable for assembled shaft support and its preparation method and application.
[0043] The technical solution in the present invention is to solve the above problems, and the overall idea is as follows:
[0044] The present invention provides a new backfill material suitable for assembled shaft support, which comprises component A and component B by weight, wherein:
[0045] Component A includes:
[0046] 10-30 parts of diphenylmethane diisocyanate;
[0047] 70-90 parts of polymethylene polyphenyl isocyanate;
[0048] Component B includes:
[0049] 40-60 parts of polyether tetraol;
[0050] 35-55 parts of polyether triol;
[0051] 1.8-2.2 parts of catalyst;
[0052] 1.8 to 2.2 parts of chain extender and crosslinking agent;
[0053] 2 to 4 parts of foam stabilizer;
[0054] 10-30 parts of plasticizer;
[0055] 5 to 10 parts of foaming agent.
[0056] In a preferred embodiment, the weight ratio of component A to component B is 1:1. In actual construction operations, there are a large number of old models of foaming machines. Such foaming machines cannot adjust the flow of components A and B, and can only achieve flow control by timing. The actual operation is cumbersome, with poor precision and large errors. In order to improve the universality of the present invention, reduce dependence on construction equipment and avoid the high cost caused by equipment replacement, the technical solution of the present invention is based on the most common and widely used 1:1 ratio of two-component foaming technology, and by adding plasticizers and changing the material proportions in components A and B to change the equivalent value of the effective ingredients of the components, the mass ratio of components A and B reaches 1:1, which has a more universal application scenario.
[0057] In a preferred embodiment, the molecular weight of the polyether tetraol in component B is 500, and the molecular weight of the polyether triol is 550; preferably, the polyether tetraol in component B is polyether 4110G, and the polyether triol is polyether GP-305.
[0058] The two low molecular weight polyols selected in the present invention have similar structures and similar molecular weights, and the two have good mutual solubility. The polyether triol has lower viscosity and lower functionality, while the polyether tetraol has higher viscosity and higher functionality. The combination of the two takes into account both material properties while facilitating the control of reaction activity and being easy to operate.
[0059] In a preferred embodiment, the catalyst includes one or two of dibutyltin dilaurate and 33% concentration of triethylenediamine;
[0060] The chain extending cross-linking agent is 1,4-butanediol;
[0061] The foam stabilizer is an organosilicon copolymer;
[0062] The plasticizer is dioctyl phthalate;
[0063] The foaming agent is one or two of distilled water and monofluorodichloroethane.
[0064] In the present invention, the catalyst used is used to control the synthesis speed of the material. The catalyst includes one or more of dibutyltin dilaurate and 33% concentration of triethylenediamine. This is because when the material is synthesized, it mainly involves two chemical reactions: gel reaction and foaming reaction. Only when the reaction process of the two reactions is in a good equilibrium state, the material produced has good performance. Experiments have shown that tin-based catalysts have a significant effect on promoting the gel reaction of the material, while amine catalysts have a significant catalytic effect on the foaming reaction. The reasonable combination of the two can not only control the material synthesis speed, but also optimize the pore morphology and improve the mechanical properties of the foam. Preferably, the catalyst is composed of dibutyltin dilaurate and 33% concentration of triethylenediamine in a mass ratio of 1: (0.4-0.55).
[0065] In the present invention, the chain extender crosslinking agent used is 1,4-butanediol. As a small molecule material with a binary structure, the hydroxyl contained in it can react with the isocyanate in the polyisocyanate, so as to promote the crosslinking of the long-chain carbamate groups formed by the reaction of the isocyanate and the polyol to form a spatial grid structure, thereby making the material have better mechanical properties. It was verified by the compression test that, under the premise that other conditions remain unchanged, the amount of the chain extender is within the above range, and the compressive strength of the foam is the highest, which indirectly reflects that the mesh structure of the synthetic space of the waterproof material is the best.
[0066] In the present invention, the foam stabilizer used is an organic silicon copolymer, which contains silicon-carbon bonds and is not easy to decompose during storage and transportation. At the same time, as a surfactant, it can reduce the surface tension of the B material component and improve the miscibility of the B material; secondly, in the early stage of foaming, it can promote the formation and stability of bubble nuclei and adjust the pore structure, diameter and distribution; in addition, the organic silicon copolymer can improve the stability and fluidity of the expanded foam raw material system, so that the foam density of the filling material is evenly distributed and free of voids.
[0067] By adding plasticizer dioctyl phthalate and adjusting the mixing ratio of polyol component or isocyanate component while maintaining the dosage of component A and component B at 1:1, the content of polyol is reduced to avoid excessive proportion of polyol in component B, which may lead to foam shrinkage. At the same time, the viscosity of the components can be easily adjusted to make the viscosity of the two components as close as possible, which is conducive to uniform mixing of different components. In addition, the plasticizer can be dissolved into the filling material and will not migrate, so it has little negative impact on the compressive and tensile properties of the material.
[0068] In the present invention, the foaming agent used is one or two of distilled water and monofluorodichloroethane; the foaming principle of distilled water is that the hydroxyl group in the water reacts with the isocyanate group in the polyisocyanate to generate urea groups and release carbon dioxide, thereby achieving the foaming effect. However, when only distilled water is used as a foaming agent to react with the two isocyanates in component A, the phenomenon of excessively fast bubble generation will occur, which is very likely to cause bubble loss, thereby increasing the structural brittleness and the foam density is high. Therefore, the present invention considers adding another foaming agent to mix with distilled water. Monofluorodichloroethane is a physical foaming agent, which mainly relies on the heat generated by the reaction of isocyanate and polyol to gasify and play a foaming role, but monofluorodichloroethane has a strong solvent effect, which is easy to destroy the pores and cause the foam strength to decrease. When monofluorodichloroethane and distilled water are used in combination, the purpose of synergistic enhancement can be achieved, which can not only reduce the rate of bubble generation, but also reduce the solvent effect of monofluorodichloroethane and the damage to the pore structure, thereby making the pore structure of the foaming system more complete and stable, and achieving better foaming effect.
[0069] Preferably, the foaming agent is composed of distilled water and monofluorodichloroethane in a mass ratio of 1:(5-6). When the foaming agent ratio is within this range, by comparing the yield strength, it is indirectly reflected that the pore structure of the filling material is the most complete and stable.
[0070] Another object of the present invention is to provide a method for preparing a new backfill material suitable for assembled shaft support, which specifically comprises the following steps:
[0071] Preparation of component A: Weigh diphenylmethane diisocyanate and polymethylene polyphenyl isocyanate in parts by weight, and mix them evenly at room temperature to obtain component A;
[0072] Preparation of component B:
[0073] (1) Weighing the polyether tetraol and polyether triol in component B by weight, mixing at room temperature, and drying to obtain a mixed polyether polyol;
[0074] (2) Add a catalyst, a chain extender, a cross-linking agent, a foam stabilizer, a foaming agent and a plasticizer to the mixed polyether polyol, and stir evenly at room temperature to obtain the obtained product.
[0075] In a preferred embodiment, in step (1), the drying treatment conditions are: drying at 40-60° C. for 12-24 hours, and more preferably, the drying device is a vacuum dryer. After drying under such conditions, the properties of the polyether polyol are not affected, and the internal moisture can be fully removed to avoid affecting the reaction effect when blending with other raw materials.
[0076] Another object of the present invention is to provide an application method of a new backfill material suitable for assembled shaft support, which specifically comprises the following steps:
[0077] At the construction site, component A and component B are respectively poured into a two-component foaming machine, and a mixed slurry is obtained through the foaming reaction. The mixed slurry is injected into the space between the shaft and the supporting structure through the grouting holes to foam and generate the filling material behind the shaft support.
[0078] In a preferred embodiment, the new backfill material suitable for prefabricated shaft support has an underground depth of up to 475m, a ground stress of up to 14.46MPa, a foaming temperature of 30-80°C, and the outer filling material includes one or more of metal, concrete, and rock.
[0079] In a preferred embodiment, the foaming flow rate is 20 to 24 L / min.
[0080] During the backfill construction of the assembled shaft support structure, due to the limited excavation range of the shaft, it is not suitable for the construction of large equipment. The underground engineering geological conditions of the shaft are complex, often accompanied by high ground stress, high water pressure, high humidity and other adverse geological conditions, which require early support of the shaft, short construction period, and compact and flexible operating equipment that is easy to operate. The backfill material prepared by the present invention can achieve the effects of rapid foaming reaction, high expansion rate, and fast construction speed in the range of room temperature to high temperature. Moreover, the required two-component foaming machine is small in size, flexible, and more universal, and has lower requirements for the foaming machine.
[0081] The technical solution of the present application is described in detail below through specific embodiments:
[0082] Unless otherwise specified, the technical means used in the present invention are conventional means well known to those skilled in the art, and the various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0083] In the present invention, the polymethylene polyphenyl isocyanate used, the product name is PAPI, the diphenylmethane diisocyanate, the product name is MDI, is purchased from Yantai Wanhua Polyurethane Co., Ltd.; the polyether triol used is polyether GP-305, which is purchased from Shandong Dongda Bluestar Co., Ltd.; the polyether tetraol used is polyether 4110G, 33% concentration of triethylene diamine, the product name is A33, 1,4-butanediol, triethanolamine, and dibutyltin dilaurate are all purchased from Xuzhou Yihuiyang New Materials Co., Ltd.; the monofluorodichloroethane used is purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.
[0084] In the present invention, parts by weight may be μg, mg, g, kg, or other weight units known in the art, or multiples thereof, such as 1 / 10, 1 / 100, 10 times, 100 times, etc. In the present invention, the normal temperature is 25±1°C.
[0085] Example 1
[0086] Preparation of component A: 10 g of diphenylmethane diisocyanate and 90 g of polymethylene polyphenyl isocyanate are mixed at room temperature to obtain component A;
[0087] Preparation of component B:
[0088] S1, 60g of polyether tetraol and 40g of polyether triol were mixed at room temperature, and placed in a dryer at 60°C for 24 hours to obtain a mixed polyether polyol;
[0089] S2, add 1.26g of dibutyltin dilaurate and 0.54g of A33 solution to form 1.8g of catalyst, 1.8g of chain extender cross-linking agent, 3.0g of foam stabilizer, 5g of foaming agent composed of 0.75g of water and 4.25g of monochlorodifluoroethane, and 30g of plasticizer to the dried mixed polyether polyol, stir evenly at room temperature to obtain component B;
[0090] S3. Mix component A and component B at a mass ratio of 1:1 at 30°C, use a stirrer to stir at a rate of 200 r / min for 30 seconds, and then pour into a mold to obtain a backfill material suitable for assembled shaft support.
[0091] Example 2
[0092] Preparation of component A: 30 g of diphenylmethane diisocyanate and 70 g of polymethylene polyphenyl isocyanate are mixed at room temperature to obtain component A;
[0093] Preparation of component B:
[0094] S1: 55g of polyether tetraol and 45g of polyether triol are mixed at room temperature, and placed in a dryer at 60°C for 24 hours to obtain a mixed polyether polyol;
[0095] S2, adding 1.2g of dibutyltin dilaurate and 0.6g of A33 solution to form 1.8g of catalyst, 1.8g of chain extender cross-linking agent, 3.0g of foam stabilizer, 0.75g of water and 5g of foaming agent composed of 4.25g of monochlorodifluoroethane, and 20g of plasticizer to the dried mixed polyether polyol, stirring at room temperature to obtain component B;
[0096] S3. Mix component A and component B at a mass ratio of 1:1 at 30°C, use a stirrer to stir at a rate of 200 r / min for 30 seconds, and then pour into a mold to obtain a backfill material suitable for assembled shaft support.
[0097] Example 3
[0098] Preparation of component A: 30 g of diphenylmethane diisocyanate and 70 g of polymethylene polyphenyl isocyanate are mixed at room temperature to obtain component A;
[0099] Preparation of component B:
[0100] S1: 50g of polyether tetraol and 50g of polyether triol are mixed at room temperature, and placed in a dryer at 60°C for 24 hours to obtain a mixed polyether polyol;
[0101] S2, adding 1.17g of dibutyltin dilaurate and 0.63g of A33 solution to form 1.8g of catalyst, 1.8g of chain extender crosslinker, 3.0g of foam stabilizer, 0.75g of water and 5g of foaming agent composed of 4.25g of monochlorodifluoroethane, and 10g of plasticizer to the dried mixed polyether polyol, stirring at room temperature to obtain component B;
[0102] S3. Mix component A and component B at a mass ratio of 1:1 at 30°C, use a stirrer to stir at a rate of 200 r / min for 30 seconds, and then pour into a mold to obtain a backfill material suitable for assembled shaft support.
[0103] Example 4
[0104] Preparation of component A: 30 g of diphenylmethane diisocyanate and 70 g of polymethylene polyphenyl isocyanate are mixed at room temperature to obtain component A;
[0105] Preparation of component B:
[0106] S1: 60g of polyether tetraol and 40g of polyether triol are mixed at room temperature, and placed in a dryer at 60°C for drying and dehydration for 24 hours to obtain a mixed polyether polyol;
[0107] S2, add 1.45g of dibutyltin dilaurate and 0.73g of A33 solution to form 2.2g of catalyst, 2.2g of chain extender cross-linking agent, 4.0g of foam stabilizer, 10g of foaming agent composed of 1.5g of water and 8.5g of monochlorodifluoroethane, and 20g of plasticizer to the dried mixed polyether polyol, stir evenly at room temperature to obtain component B;
[0108] S3. Mix component A and component B at a mass ratio of 1:1 at 30°C, use a stirrer to stir at a rate of 200 r / min for 30 seconds, and then pour into a mold to obtain a backfill material suitable for assembled shaft support.
[0109] Example 5
[0110] In Example 1, in step S3, the mixing temperature of component A and component B is adjusted to 60° C., and the rest is completely consistent with Example 3.
[0111] Effect example
[0112] The technical effects of the backfill materials obtained in test examples 1-8 are as follows:
[0113] Measure the density of materials according to GB / T 6343-2009;
[0114] Measure the setting time of materials according to JC / T 2041-2010;
[0115] Measure the tensile strength of materials according to GB / T9641-1998;
[0116] Measure the 10% compressive strength of the material according to GB / T8813-2020;
[0117] Determine the material permeability coefficient based on the field test of the borehole water pressure test in the Engineering Geology Handbook;
[0118] The expansion force of the material with 110% interference is tested using a self-developed device.
[0119] The specific test results are shown in Table 1:
[0120] Table 1
[0121]
[0122] It can be seen from Table 1 that under the conditions of room temperature of 30°C and conventional operating temperature of 60°C, the back filling materials prepared by the present invention have the characteristics of faster reaction time, stronger mechanical properties, lower expansion force, and lower density, and the solidification time is shorter when reacting at high temperature. The raw materials used are low-cost and easy to purchase, and the production process is simple and safe, easy to process, and has low requirements for equipment and energy consumption, which can further reduce the preparation cost and improve the economic benefit. The prepared material is particularly suitable as a back filling material for assembled shaft support due to its excellent performance, which can tightly connect metal materials, concrete materials and rocks.
[0123] Comparative Example 1
[0124] Preparation of component A: 30 g of diphenylmethane diisocyanate and 70 g of polymethylene polyphenyl isocyanate are mixed at room temperature to obtain component A;
[0125] Preparation of component B:
[0126] S1: 50g of polyether tetraol and 50g of polyether triol are mixed at room temperature, and placed in a dryer at 60°C for 24 hours to obtain a mixed polyether polyol;
[0127] S2, adding 1.2g of dibutyltin dilaurate and 0.6g of A33 solution to the dried mixed polyether polyol to form 1.8g of catalyst, adding different amounts of chain extender cross-linking agent, 3g of foam stabilizer, 0.75g of water and 4.25g of monochlorodifluoroethane to form 5g of foaming agent, and 10g of plasticizer according to Table 2, stirring evenly at room temperature to obtain component B;
[0128] S3. Mix component A and component B at a mass ratio of 1:1 at 30°C, stir quickly for 1 minute and pour into a mold to obtain a backfill material suitable for assembled shaft support.
[0129] The test results are shown in Table 2:
[0130] Table 2
[0131] Chain extender crosslinking agent dosage / g 10% compressive strength / MPa 0.6 1.13 1.2 1.20 1.8 1.22 2.4 1.19 3.0 1.11
[0132] As shown in Table 2, as the amount of chain extender cross-linking agent increases, the yield strength of the material increases first and then decreases. This is because as the amount of chain extender cross-linking agent increases, the proportion of hard segments in the molecular chain of the filling material foam increases, the number of hydrogen bonds increases, the intermolecular force increases, and its yield strength increases. When the amount of chain extender cross-linking agent is too large, the uniformity of the hard segment distribution in the soft segment of the material elastomer molecular chain decreases, resulting in a decrease in its mechanical properties.
[0133] Comparative Example 2
[0134] Preparation of component A: 30 g of diphenylmethane diisocyanate and 70 g of polymethylene polyphenyl isocyanate are mixed at room temperature to obtain component A;
[0135] Preparation of component B:
[0136] S1: 50g of polyether tetraol and 50g of polyether triol are mixed at room temperature, and placed in a dryer at 60°C for 24 hours to obtain a mixed polyether polyol;
[0137] S2, 1.2g of dibutyltin dilaurate and 0.6g of A33 solution were added to the dried mixed polyether polyol to form 1.8g of catalyst and 1.8g of chain extender crosslinker, and different amounts of foam stabilizer, 0.75g of water and 4.25g of monochlorodifluoroethane were added according to Table 3. 5g of foaming agent and 10g of plasticizer were added, and stirred evenly at room temperature to obtain component B;
[0138] S3. Mix component A and component B at a mass ratio of 1:1 at 30°C, stir quickly for 1 minute and pour into a mold to obtain a backfill material suitable for assembled shaft support.
[0139] The test results are shown in Table 3:
[0140] Table 3
[0141] Foam stabilizer dosage / g <![CDATA[Density Kg / m 3 > 10% compressive strength / MPa 1 0.1451 0.97 2 0.1434 1.13 3 0.1423 1.22 4 0.1413 1.11 5 0.1408 1.02
[0142] As shown in Table 3, as the amount of foam stabilizer increases, the density of the material decreases, and the yield strength increases first and then decreases. This is because the foam stabilizer can reduce the surface tension of the raw material, promote the formation of bubble nuclei, reduce bubble loss, and optimize the pore structure, so the foam density increases and the yield strength increases. However, when the amount of foam stabilizer accounts for more than 3% of the polyether polyol, the flexible silicone molecular chain causes the rigidity of the foam to decrease, and the yield strength also decreases.
[0143] Comparative Example 3
[0144] Preparation of component A: 30 g of diphenylmethane diisocyanate and 70 g of polymethylene polyphenyl isocyanate are mixed at room temperature to obtain component A;
[0145] Preparation of component B:
[0146] S1: 50g of polyether tetraol and 50g of polyether triol are mixed at room temperature, and placed in a dryer at 60°C for 24 hours to obtain a mixed polyether polyol;
[0147] S2, adding 1.2g of dibutyltin dilaurate and 0.6g of A33 solution to form 1.8g of catalyst, 1.8g of chain extender crosslinker, 3.0g of foam stabilizer, 0.75g of water and 5g of foaming agent composed of 4.25g of monochlorodifluoroethane, without adding plasticizer, and stirring at room temperature to obtain component B;
[0148] S3. Mix component A and component B at a mass ratio of 1:1 at 30°C, stir quickly for 1 minute and pour into a mold to obtain a backfill material suitable for assembled shaft support.
[0149] The back filling material prepared under the experimental conditions showed obvious shrinkage after curing and molding, and its diameter was reduced by nearly 1 / 3. This was because no plasticizer was added and the mass ratio of components A and B was 1:1, which resulted in too large a proportion of polyol, increased proportion of soft segments in the foam, and reduced mechanical strength of the material. After curing, the pores broke and the bubbles escaped, causing the back filling material to shrink in volume and shrink.
[0150] Comparative Example 4
[0151] Preparation of component A: 30 g of diphenylmethane diisocyanate and 70 g of polymethylene polyphenyl isocyanate are mixed at room temperature to obtain component A;
[0152] Preparation of component B:
[0153] S1: 50g of polyether tetraol and 50g of polyether triol are mixed at room temperature, and placed in a dryer at 60°C for 24 hours to obtain a mixed polyether polyol;
[0154] S2, adding 0.6g of dibutyltin dilaurate and 1.2g of A33 to form 1.8g of catalyst, 1.8g of chain extender crosslinker, 3.0g of foam stabilizer, 5g of foaming agent composed of 0.75g of water and 4.25g of monochlorodifluoroethane, and 10g of plasticizer to the dried mixed polyether polyol, stirring evenly at room temperature to obtain component B;
[0155] S3. Mix component A and component B at a mass ratio of 1:1 at 30°C, stir quickly for 1 minute and pour into a mold to obtain a backfill material suitable for assembled shaft support.
[0156] Under the experimental conditions, the ratio of dibutyltin dilaurate and A33 was seriously unbalanced, and the resulting filling material had coarse pores, which made it impossible to manufacture tensile specimens, and powdered failure occurred when subjected to force. This was because the amount of A33 used was large and the amount of dibutyltin dilaurate used was small, resulting in a slower gel reaction than a foaming reaction, that is, the formed gel could not carry bubbles, resulting in a large number of bubbles escaping or agglomerating, which in turn increased the material density, coarse pores, and easy powder failure.
[0157] Comparative Example 5
[0158] Preparation of component A: 30 g of diphenylmethane diisocyanate and 70 g of polymethylene polyphenyl isocyanate are mixed at room temperature to obtain component A;
[0159] Preparation of component B:
[0160] S1: 50g of polyether tetraol and 50g of polyether triol are mixed at room temperature, and placed in a dryer at 60°C for 24 hours to obtain a mixed polyether polyol;
[0161] S2, add 1.2g of dibutyltin dilaurate and 0.6g of A33 solution to the dried mixed polyether polyol to form 1.8g of catalyst, 1.8g of chain extender crosslinker, 3.0g of foam stabilizer, and prepare 5g of foaming agent and 10g of plasticizer with water and monochlorodifluoroethane according to Table 4, stir evenly at room temperature to obtain component B;
[0162] S3. Mix component A and component B at a mass ratio of 1:1 at 30°C, stir quickly for 1 minute and pour into a mold to obtain a backfill material suitable for assembled shaft support.
[0163] The test results are shown in Table 4:
[0164] Table 4
[0165] Water: Chlorodifluoroethane <![CDATA[Density Kg / m 3 > 10% compressive strength / MPa 1:3 0.1405 0.98 1:4 0.1412 1.11 1:5 0.1423 1.22 1:6 0.1431 1.18 1:7 0.1444 1.01
[0166] As can be seen from Table 4, with the increase of the proportion of chlorodifluoroethane, the density of the material increases, and the yield strength first increases and then decreases. This is because chlorodifluoroethane has a strong solvent effect, which will destroy the pores, increase the gas escape amount, and increase the density. When water is used as a chemical foaming agent, the bubble generation rate is faster when the water content is high, and the generated foam is brittle, the foam morphology is poor, and the mechanical properties are poor. As the proportion of chlorodifluoroethane gradually increases, chlorodifluoroethane gasification absorbs heat, which to a certain extent reduces the speed at which water and isocyanate produce carbon dioxide, optimizes the pore morphology, and increases the yield strength. However, when the content of chlorodifluoroethane is too high, the pores are broken in large quantities, and the yield strength is reduced instead. Therefore, in the present invention, the ratio of water to chlorodifluoroethane in the foaming agent is designed to be 1: (5-6).
[0167] The foregoing description of specific exemplary embodiments of the present invention is for the purpose of illustration and demonstration. These descriptions are not intended to limit the present invention to the precise form disclosed, and it is clear that many changes and variations can be made based on the above teachings. The purpose of selecting and describing the exemplary embodiments is to explain the specific principles of the present invention and its practical application, so that those skilled in the art can realize and utilize various different exemplary embodiments of the present invention and various different selections and changes. The scope of the present invention is intended to be limited by the claims and their equivalents.
Claims
1. A backfill material suitable for assembled shaft support, It is characterized in that Calculated by weight, it includes component A and component B, wherein: Component A includes: 10-30 parts of diphenylmethane diisocyanate; 70-90 parts of polymethylene polyphenyl isocyanate; Component B includes: 40-60 parts of polyether tetraol; 35-55 parts of polyether triol; 1.8-2.2 parts of catalyst; 1.8-2.2 parts of chain extension crosslinking agent; 2~4 parts of foam stabilizer; Plasticizer 10~30 parts; 5-10 parts of foaming agent; Wherein, the weight ratio of component A to component B is 1:1; The chain extending cross-linking agent is 1,4-butanediol; The foam stabilizer is an organosilicon copolymer; The catalyst is composed of dibutyltin dilaurate and 33% triethylenediamine in a mass ratio of 1: (0.4-0.55); The foaming agent is composed of distilled water and monofluorodichloroethane in a mass ratio of 1: (5-6).
2. The backfill material suitable for assembled shaft support as claimed in claim 1, It is characterized in that The molecular weight of the polyether tetraol in component B is 500, and the molecular weight of the polyether triol is 550.
3. The backfill material suitable for assembled shaft support as claimed in claim 2, It is characterized in that The polyether tetraol in component B is polyether 4110G, and the polyether triol is polyether GP-305.
4. A method for preparing a backfill material suitable for assembled shaft support according to any one of claims 1 to 3, It is characterized in that The following steps are involved: Preparation of component A: Weigh diphenylmethane diisocyanate and polymethylene polyphenyl isocyanate in parts by weight, and mix them evenly at room temperature to obtain component A; Preparation of component B: (1) Weighing the polyether tetraol and polyether triol in component B according to weight, mixing at room temperature, and drying to obtain a mixed polyether polyol; (2) Add a catalyst, a chain extender, a cross-linking agent, a foam stabilizer, a foaming agent and a plasticizer to the mixed polyether polyol and stir evenly at room temperature to obtain the obtained product.
5. The method for preparing the backfill material suitable for assembled shaft support according to claim 4, It is characterized in that In step (1), the drying treatment conditions are: drying at 40-60° C. for 12-24 hours.
6. A method for using the backfill material suitable for assembled shaft support according to any one of claims 1 to 3 or the backfill material obtained by the preparation method according to any one of claims 4 to 5, It is characterized in that The following steps are involved: At the construction site, component A and component B are respectively poured into a two-component foaming machine, and a mixed slurry is obtained through the foaming reaction. The mixed slurry is injected into the space between the shaft and the supporting structure through the grouting holes to foam and generate the filling material behind the shaft support.
7. The application method according to claim 6, It is characterized in that The backfill material suitable for assembled shaft support can reach an underground depth of 475m, a ground stress of 14.46MPa, a foaming temperature of 30-80°C, and the outer filling material includes one or more of metal, concrete, and rock.
Citation Information
Patent Citations
High-fire-retardant polyurethane filling foam for door and window profiles and preparation method thereof
CN105294982A
Polyurethane composite material and polyurethane heat-preserving material prepared therefrom
CN106046317A