A method for reducing the crystallinity of polylactic acid
The crystallinity of polylactic acid is reduced through pretreatment and ball milling treatment, and the magnetic material is wrapped in silica for ball milling treatment, which solves the problem of slow degradation speed due to high crystallinity of polylactic acid, and achieves rapid degradation of polylactic acid in soil. in food packaging and other fields.
Patent Information
- Application Number
- CN202211509427.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-29
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-11-29
AI Technical Summary
The high crystallinity of polylactic acid leads to its slow degradation rate in soil, limiting its use in more applications.
By combining pretreatment and ball milling treatment, the crystallinity of polylactic acid is reduced, including ball milling using silica-encapsulated magnetic material, breaking up the structure of the PLA and increasing its microbial degradation rate in the soil.
It effectively reduces the crystallinity of polylactic acid, makes it degraded faster in the soil, improves the biodegradation rate, and is suitable for a wider range of fields such as food packaging and other degradable materials.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of polylactic acid modification, and more specifically, relates to a method for reducing the crystallinity of polylactic acid. Background Art
[0002] Polylactic acid (PLA) is an aliphatic polyester, which is a renewable plant resource made from corn, sugar cane, etc. The raw materials of polylactic acid are green and pollution-free, and the sources are extensive, with abundant production reserves. After use, polylactic acid can be quickly degraded into carbon dioxide and water using compost. However, the crystallinity of L-polylactic acid is about 37%. Although it can be completely degraded in the soil, the soil degradation rate of high-crystallinity polylactic acid can be further improved, and low-crystallinity PLA can be completely degraded in the soil in a shorter time.
[0003] Therefore, the present invention designs a method for reducing the crystallinity of polylactic acid, so that it can be applied in a wider range of fields. Summary of the invention
[0004] In order to overcome the above disadvantages and improve the problem of high crystallinity of pure PLA, the present invention reduces the crystallinity of PLA by combining pretreatment and physical treatment, so that PLA with low crystallinity can be degraded faster in soil.
[0005] The object of the present invention is achieved in the following ways:
[0006] A method for reducing the crystallinity of polylactic acid, the method comprising pretreatment, ball milling and recovery of polylactic acid for tableting; wherein the ball milling material used in the ball milling is a magnetic material wrapped in silica, the ball milling time is 0.5-1h, and the ball milling speed is 300-350rpm.
[0007] Preferably, the pretreatment step is to take 1 part by weight of polylactic acid powder, add 4-6 parts by weight of precooled acetone, stir for 30-60 minutes, then add 8-10 parts by weight of 35% concentrated hydrochloric acid, stir on a magnetic stirrer until it becomes a colorless paste, after stirring, adjust the pH to neutral, continue heating and stirring at 70-80°C for 2-3 hours, cool to room temperature, add 10-12 parts by weight of precooled 50% ethanol, stir quickly and mix thoroughly, leave at 4°C overnight, cool and precipitate polylactic acid, filter, collect the polylactic acid, and rinse repeatedly with deionized water 3-5 times.
[0008] Preferably, the polylactic acid powder is obtained by crushing polylactic acid solid particles and sieving to obtain 80 mesh powder.
[0009] Preferably, the pH is adjusted using 5M sodium hydroxide.
[0010] Preferably, the stirring time on the magnetic stirrer is 2-4 hours.
[0011] Preferably, the precooling temperature is 4° C. Preferably, the ball milling treatment is to dry the pretreated polylactic acid, crush it, sieve out 100 mesh powder, take 1 weight part of polylactic acid powder, add 5-8 weight parts of 200 μm silicon dioxide-wrapped magnetic material, mix them in a ball mill grinding tank, and ball mill them. After the ball milling is completed, the ferroferric oxide balls are recovered with a strong magnet and can be recycled.
[0012] Preferably, the silicon dioxide-coated magnetic material is a small iron oxide ball with a silicon dioxide outer layer.
[0013] Preferably, circulating water is introduced during the ball milling process.
[0014] Preferably, the polylactic acid is recycled and pressed into sheets by remelting the ball-milled polylactic acid into 1-2 mm polylactic acid sheets.
[0015] The method of the present invention specifically comprises the following steps:
[0016] 1. PLA pretreatment
[0017] Weigh PLA solid particles, crush them, and sieve out 80 mesh powder for later use. Take 1 part by weight of PLA powder, add 4-6 parts by weight of pre-cooled acetone, and stir for 30-60 minutes. Then add 8-10 parts by weight of 35% concentrated hydrochloric acid, and stir on a magnetic stirrer for 2-4 hours until it becomes a colorless paste. After stirring, adjust the pH to neutral with 5M sodium hydroxide solution, and continue heating (70-80°C) and stirring for 2-3 hours. Cool to room temperature, add 10-12 parts by weight of pre-cooled 50% ethanol, stir quickly and mix thoroughly, place at 4°C overnight to allow PLA to cool and precipitate, filter and collect PLA, and rinse PLA repeatedly with deionized water 3-5 times.
[0018] 2. Ball milling
[0019] The pretreated PLA is dried, crushed again, and sieved to obtain a 100-mesh powder. Take 1 part by weight of the treated PLA, add 5-8 parts by weight of 200 μm ferroferric oxide balls with an outer layer of silicon dioxide. Mix them in a ball mill grinding tank, connect circulating water to prevent melting due to excessive temperature, ball milling time is 0.5-1h, and ball milling speed is 300-350rpm.
[0020] 3. PLA recycling and tableting
[0021] The ball-milled PLA is re-melted and pressed into 1-2 mm PLA sheets.
[0022] The obtained PLA sheets were subjected to the following biodegradation experiment: the treated PLA sheets were cut into 1 cm*1 cm sheets and weighed and recorded, and buried at a depth of 15-20 cm. The degradation cycle was 90 days, and the materials were collected every 30 days, dried, and the total weight was weighed.
[0023] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0024] 1. Through specific pretreatment, the structure of PLA can be effectively broken up and the crystallinity of PLA can be initially reduced;
[0025] 2. Further adding ball milling treatment can more effectively reduce the crystallinity of PLA and play a complementary role;
[0026] 3. The material used for ball milling is a magnetic material wrapped in silica, which can be effectively ball milled and can be directly recycled through magnets;
[0027] Therefore, the PLA material with low crystallinity of the present invention can be degraded more quickly by microorganisms in the soil. DETAILED DESCRIPTION
[0028] The present invention is further explained below by specific examples:
[0029] Embodiment 1:
[0030] 1. PLA pretreatment
[0031] Weigh PLA solid particles, crush them, and sieve out 80 mesh powder. Take 1 part by weight of PLA powder, add 4 parts by weight of pre-cooled acetone, and stir for 30 minutes. Then add 8 parts by weight of 35% concentrated hydrochloric acid, and stir on a magnetic stirrer for 2 hours until it becomes a colorless paste. After stirring, adjust the pH to neutral with 5M sodium hydroxide solution, and continue heating (70°C) and stirring for 2 hours. Cool to room temperature, add 10 parts by weight of pre-cooled 50% ethanol, stir quickly and mix thoroughly, place at 4°C overnight to allow PLA to cool and precipitate, filter and collect PLA, and rinse PLA repeatedly with deionized water 3 times.
[0032] 2. Ball milling
[0033] The pretreated PLA is dried, crushed again, and sieved to obtain a 100-mesh powder. Take 1 part by weight of the treated PLA and add 5 parts by weight of 200 μm ferroferric oxide balls with an outer layer of silicon dioxide. Mix them in a ball mill grinding tank and connect to circulating water to prevent melting due to excessive temperature. The ball milling time is 0.5 hours and the ball milling speed is 300 rpm. After the ball milling is completed, the ferroferric oxide balls are recovered with a strong magnet and can be recycled.
[0034] 3. PLA recycling and tableting
[0035] The ball-milled PLA was re-melted and pressed into 1 mm PLA sheets.
[0036] 4. Biodegradation experiment of PLA
[0037] The treated PLA sheets were cut into 1cm*1cm sheets and weighed and recorded, and buried at a depth of 15cm. The degradation cycle was 90 days, and the materials were collected every 30 days, dried, and weighed.
[0038] Embodiment 2:
[0039] 1. PLA pretreatment
[0040] Weigh PLA solid particles, crush them, and sieve out 80 mesh powder. Take 1 part by weight of PLA powder, add 4 parts by weight of pre-cooled acetone, and stir for 60 minutes. Then add 10 parts by weight of 35% concentrated hydrochloric acid, and stir on a magnetic stirrer for 2 hours until it becomes a colorless paste. After stirring, adjust the pH to neutral with 5M sodium hydroxide solution, and continue heating (80°C) and stirring for 2-3 hours. Cool to room temperature, add 12 parts by weight of pre-cooled 50% ethanol, stir quickly and mix thoroughly, and place at 4°C overnight to allow PLA to cool and precipitate, filter and collect PLA, and rinse PLA repeatedly with deionized water 5 times.
[0041] 2. Ball milling
[0042] The pretreated PLA is dried, crushed again, and sieved to obtain a 100-mesh powder. Take 1 part by weight of the treated PLA and add 5 parts by weight of 200 μm ferroferric oxide balls with an outer layer of silicon dioxide. Mix them in a ball mill grinding tank and connect to circulating water to prevent melting due to excessive temperature. The ball milling time is 0.5 hours and the ball milling speed is 300 rpm. After the ball milling is completed, the ferroferric oxide balls are recovered with a strong magnet and can be recycled.
[0043] 3. PLA recycling and tableting
[0044] The ball-milled PLA was re-melted and pressed into 1 mm PLA sheets.
[0045] 4. Biodegradation experiment of PLA
[0046] The treated PLA sheets were cut into 1cm*1cm sheets and weighed and recorded, and buried at a depth of 20cm. The degradation cycle was 90 days, and the materials were collected every 30 days, dried, and weighed.
[0047] Embodiment 3:
[0048] 1. PLA pretreatment
[0049] Weigh PLA solid particles, crush them, and sieve out 80 mesh powder. Take 1 part by weight of PLA powder, add 6 parts by weight of pre-cooled acetone, and stir for 60 minutes. Then add 10 parts by weight of 35% concentrated hydrochloric acid, and stir on a magnetic stirrer for 4 hours until it becomes a colorless paste. After stirring, adjust the pH to neutral with 5M sodium hydroxide solution, and continue heating (80°C) and stirring for 3 hours. Cool to room temperature, add 12 parts by weight of pre-cooled 50% ethanol, stir quickly and mix thoroughly, place at 4°C overnight to allow PLA to cool and precipitate, filter and collect PLA, and rinse PLA repeatedly with deionized water 5 times.
[0050] 2. Ball milling
[0051] Dry the pretreated PLA, crush it again, and sieve out 100 mesh powder. Take 1 part by weight of the treated PLA and add 5-8 parts by weight of 200μm ferroferric oxide balls with silicon dioxide wrapped on the outer layer. Mix them in the grinding tank of the ball mill, connect to circulating water to prevent melting due to excessive temperature, ball milling time is 1h, ball milling speed is 350rpm. After the ball milling is completed, the ferroferric oxide balls are recovered with a strong magnet and can be recycled.
[0052] 3. PLA recycling and tableting
[0053] The ball-milled PLA was re-melted and pressed into 1 mm PLA sheets.
[0054] 4. Biodegradation experiment of PLA
[0055] The treated PLA sheets were cut into 1cm*1cm sheets and weighed and recorded, and buried at a depth of 20cm. The degradation cycle was 90 days, and the materials were collected every 30 days, dried, and weighed.
[0056] Comparative Example 1:
[0057] Pure PLA material (without any treatment)
[0058] Comparative Example 2:
[0059] PLA material without pretreatment (without pretreatment, the remaining steps and conditions are the same as those in Example 1 of the present invention)
[0060] Comparative Example 3:
[0061] PLA material without ball milling (without ball milling, the remaining steps and conditions are the same as those in Example 2 of the present invention) Comparative Example 4:
[0062] Ball milling speed 500 rpm (after ball milling, the remaining steps and conditions are the same as those in Example 3 of the present invention)
[0063] Product of Example 1 of the present invention: PLA material prepared in Example 1 of the present invention
[0064] Product of Example 2 of the present invention: PLA material prepared in Example 2 of the present invention
[0065] Product of Example 3 of the present invention: PLA material prepared in Example 3 of the present invention
[0066] Crystallinity test: The test was conducted using a differential scanning calorimeter (DSC) in a nitrogen atmosphere with a heating / cooling rate of 10°C / min and a temperature range of 30-200°C. The relative crystallinity of the material was calculated using the heating melting curve.
[0067] Table 1 Performance test table
[0068] Test indicators Crystallinity % 90d biodegradation rate % Comparative Example 1 38 83 Comparative Example 2 25 86 Comparative Example 3 22 89 Comparative Example 4 28 87 Example 1 14 98 Example 2 13 98 Example 3 16 97
[0069] The results show that the PLA material prepared by the preparation method of the present invention has an improved biodegradation rate in soil due to the effective reduction of the crystallinity of PLA. Therefore, the modified PLA prepared by the preparation method of the present invention can be used in degradable fields such as food packaging.
[0070] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.
Claims
1. A method for reducing the crystallinity of polylactic acid, characterized in that The method comprises pretreatment, ball milling and polylactic acid recovery and tableting; wherein the ball milling material used in the ball milling is a magnetic material wrapped in silicon dioxide, the ball milling time is 0.5-1 h, and the ball milling speed is 300-350 rpm; The pretreatment step is to take 1 part by weight of polylactic acid powder, add 4-6 parts by weight of precooled acetone, stir for 30-60 minutes, then add 8-10 parts by weight of 35% concentrated hydrochloric acid, stir on a magnetic stirrer until it becomes a colorless paste, adjust the pH to neutral after stirring, continue heating and stirring at 70-80°C for 2-3 hours, cool to room temperature, add 10-12 parts by weight of precooled 50% ethanol, stir quickly and mix thoroughly, leave overnight at 4°C, cool and precipitate polylactic acid, filter, collect polylactic acid, and rinse repeatedly with deionized water for 3-5 times, wherein the precooling temperature is 4°C; The ball milling treatment is to dry the pretreated polylactic acid, crush it, sieve out 100 mesh powder, add 5-8 weight parts of 200 μm silica-coated magnetic material to 1 weight part of polylactic acid powder, mix them in a ball mill grinding jar, and ball mill them.
2. The method for reducing the crystallinity of polylactic acid according to claim 1, characterized in that The polylactic acid powder is obtained by crushing polylactic acid solid particles and sieving 80-mesh powder.
3. The method for reducing the crystallinity of polylactic acid according to claim 1, characterized in that The pH is adjusted using 5 M sodium hydroxide.
4. The method for reducing the crystallinity of polylactic acid according to claim 1, characterized in that The stirring time on the magnetic stirrer is 2-4 h.
5. The method for reducing the crystallinity of polylactic acid according to claim 1, characterized in that The silicon dioxide-wrapped magnetic material is a small iron oxide ball with a silicon dioxide outer layer.
6. The method for reducing the crystallinity of polylactic acid according to claim 1, characterized in that Circulating water is introduced into the ball milling process.
7. The method for reducing the crystallinity of polylactic acid according to claim 1, characterized in that The polylactic acid recycling and tableting is to melt the ball-milled polylactic acid again and press it into 1-2 mm polylactic acid sheets.
Citation Information
Patent Citations
Fast-crystallization and high-crystallinity polylactic acid modification method
CN110760172A
Modified polylactic acid with gradient crystallinity and preparation method and application thereof
CN114410082A
Polylactic acid composition
US20170015806A1