A UV moisture dual-curing reactive polyurethane hot melt adhesive and preparation method thereof
Through the combination technology of UV moisture dual-curing reactive polyurethane hot melt adhesive, the photoinitiator and moisture reaction are used to form a high-strength network chain structure and urethane group, which solves the problem of existing UV adhesives in areas where light is not available. Solving the problems of low strength and allergenic monomers, high initial and final bonding strength is achieved to meet the environmental protection and high reliability requirements in the field of electronic assembly.
Patent Information
- Application Number
- CN202211554880.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-06
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-12-06
AI Technical Summary
Existing UV adhesives have low strength in areas not exposed to light and contain allergenic monomers, making it difficult to meet the needs for high bonding strength and environmental protection and non-toxicity. In particular, there are deficiencies in production efficiency and environmental protection requirements in the field of electronic assembly. .
UV moisture dual-curing reactive polyurethane hot melt adhesive is used by combining crystalline polyester polyol, amorphous polyester polyol, polyol with acrylic ester, acrylic resin, petroleum resin, silane coupling agent and catalyst. The photoinitiator and moisture curing reaction form a network chain structure and a urethane group and urea structure to achieve high initial and final bonding strength.
High bonding strength is obtained immediately after illumination, and the bonding strength is further improved through moisture curing to ensure high curing strength under no-light conditions, meeting the environmental protection and high reliability needs of the electronic packaging field.
Smart Images

Figure BDA0003982533020000071 
Figure BDA0003982533020000081
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of reactive polyurethane hot melt adhesives, and in particular relates to a UV-moisture dual-curing reactive polyurethane hot melt adhesive and a preparation method thereof. Background Art
[0002] As the electronics industry pays more and more attention to improving production efficiency, UV glue and reactive polyurethane hot melt adhesive have gradually become mainstream in electronic assembly. UV glue can be quickly cured by ultraviolet light or visible light. Reactive polyurethane hot melt adhesive is solid at room temperature, melts when heated, and is applied when it becomes a liquid or fluid state. It contacts the second bonding substrate before cooling, and can form a solid glue with a certain bonding strength after cooling, and then further solidifies and cross-links with moisture in the air, and finally obtains a higher bonding strength. And reactive polyurethane hot melt adhesive can form a glue line as narrow as less than 0.5mm, with the advantages of low odor, low volatility, high strength, high reliability, and fast positioning bonding.
[0003] However, as people's awareness of environmental protection increases and reports of skin irritation caused by allergenic monomers contained in the main acrylic ester type UV adhesive increase, the electronic consumer field is gradually moving towards reactive polyurethane hot melt adhesives. However, the characteristic of UV adhesives that can be quickly fixed by light is irreplaceable. Although environmentally friendly and non-toxic reactive polyurethane hot melt adhesives can obtain a certain strength through cooling of crystalline substances or high softening point substances in the formula, it often takes 10-20 minutes to maintain pressure and fix, which reduces production efficiency.
[0004] UV moisture dual-curing UV adhesives are now available on the market, but some still contain allergenic monomers, and some have low strength in areas where light cannot reach, and can only maintain a non-flowing state, affecting practical applications.
[0005] Therefore, there is a need for a colloid that can achieve a higher initial strength after exposure to light to meet the initial transportation requirements; can further improve the bonding strength through moisture curing to meet the requirements of high adhesion and high reliability; at the same time, can still maintain a high strength in areas where light cannot reach; and is environmentally friendly and free of allergenic monomers. Summary of the invention
[0006] In view of the above-mentioned deficiencies in the prior art, the present invention provides a UV-moisture dual-curing reactive polyurethane hot melt adhesive and a preparation method thereof.
[0007] The specific technical solutions of the present invention are as follows:
[0008] The first object of the present invention is to provide a UV moisture dual-curing reactive polyurethane hot melt adhesive, comprising the following components in parts by weight:
[0009] Crystalline polyester polyol 15-45 parts, non-crystalline polyester polyol 15-30 parts, polyether polyol 15-30 parts, polyol with acrylate 5-40 parts, acrylic resin 5-20 parts, petroleum resin 5-20 parts, diisocyanate 10-30 parts, silane coupling agent 0.05-0.5 parts, catalyst 0.05-0.5 parts, photoinitiator 0.5-3 parts
[0010] The UV-moisture dual-curing reactive polyurethane hot melt adhesive of the present invention obtains a high bonding strength immediately after being irradiated with UV light, and the strength continues to increase in subsequent contact with moisture. It has the characteristics of rapid bonding and fixing of UV adhesive and high reliability of polyurethane hot melt adhesive, and has a high curing strength when cured under lightless conditions.
[0011] Furthermore, the synthesis method of the polyol with acrylate is as follows: dehydrating a trifunctional polyol, heating it with isocyanoethyl methacrylate (MOI) or isocyanoethyl acrylate (AOI) to obtain the polyol, and adding a proper amount of phenothiazine during the reaction; the molar ratio of the dehydrated trifunctional polyol to MOI or AOI is 1:(1-2); the amount of phenothiazine added is 0.005-0.02 g per mol of the trifunctional polyol, and the polyol with acrylate needs to be kept in a sealed container to isolate moisture for standby use.
[0012] The present invention adds polyol with acrylate, and after being illuminated, double bonds between acrylate groups are added to form a network chain structure, and at the same time, the crystallized diol crystallizes and cools, which can also provide a certain cohesive strength. With moisture curing, the glue forms a large number of urethane groups and urea structures to improve the bonding and cohesive strength. After the polyol with acrylate reacts with polyisocyanate, it can participate in both light and moisture curing, so that it still has a high strength under no light conditions.
[0013] Furthermore, the trifunctional polyol is a polyol having three functional groups, and all polyols with a functionality of 3 belong to the trifunctional polyol referred to herein, including polyether triol, polycaprolactone triol or castor oil triol, including polyether 307, polyether N3600, and dasiro polycaprolactone 305T.
[0014] Furthermore, the crystalline polyester polyol is preferably one or two of Evonik Dynacoll 7330, Dynacoll 7340, Dynacoll 7360, Dynacoll 7380 or Dynacoll 7390.
[0015] Furthermore, the non-crystalline polyester polyol is preferably one or two of Evonik Dynacoll 7250, Evonik Dynacoll 7255, and Asahikawa Chemical FLP2000N.
[0016] Furthermore, the polyether polyol is one or two of polypropylene glycol, polytetramethylene glycol or polymethyltetramethylene glycol, such as PPG1000, PPG2000, PTMG1000, PTMG2000, etc. The polyether polyol used in the present invention is a polyol with a polyether structure as the main repeating chain link, which can provide flexibility.
[0017] Furthermore, the acrylic acid ester is a polymer or copolymer of acrylic acid or methacrylic acid alkyl ester, such as one or more of WK502, WK501, BR113, BR115, ELVACITE 2044, and ELVACITE 2927.
[0018] Furthermore, the petroleum resin is C5 petroleum resin, C9 petroleum resin, polystyrene resin, aliphatic hydrocarbon modified polystyrene resin, such as one or more of Eastman 3100, 3120, 3140.
[0019] Furthermore, the diisocyanate is diphenylmethane-4,4'-diisocyanate (MDI).
[0020] Furthermore, the silane coupling agent is one or more of KH560, KH550, y-9669, A-189, mercaptopropyltrimethoxysilane, and ALINK597.
[0021] Furthermore, the catalyst includes one or two of dibutyltin diisocyanate, stannous octoate, triethylenediamine, and bismorpholinyl ethyl ether. The addition of the catalyst adjusts the synthesis reaction and the final curing speed.
[0022] Furthermore, the photoinitiator is one or more of the photoinitiators TPO, TPO-L, 184, 907 or 819. The photoinitiator can be any photoinitiator with good compatibility, which can be any component that is stable in the absence of light and absorbs energy to initiate free radical polymerization under light.
[0023] The second object of the present invention is to provide a method for preparing a UV-moisture dual-curing reactive polyurethane hot melt adhesive.
[0024] Crystalline polyester polyol, non-crystalline polyester polyol, polyether polyol, polyol with acrylate, acrylic resin, petroleum resin are vacuum dehydrated at 110-150°C and less than -0.095MPa for 1.5-3h. After dehydration, the temperature is lowered to 90-110°C, diisocyanate is added, the temperature is raised to 110-120°C and the reaction is continued for 0.5-1h, and then a silane coupling agent, a catalyst, and a photoinitiator are added and stirred for 0.5-3h. The vacuum is broken, the material is discharged, and sealed and packaged to obtain a UV-moisture dual-curable reactive polyurethane hot melt adhesive.
[0025] The beneficial effects of the present invention are:
[0026] The UV moisture dual-curing reactive polyurethane hot melt adhesive prepared by the present invention is added with a polyol with acrylate, and after being irradiated with light, double bonds between acrylate groups are added to form a network chain structure, and at the same time, the crystallized diol crystallizes and cools, which can also provide a certain cohesive strength; at the same time, in the subsequent contact with moisture, as the moisture solidifies, the glue forms a large number of carbamate groups and urea structures to improve the bonding and cohesive strength, and the strength continues to increase; it has excellent initial and final bonding strength. After the polyol with acrylate reacts with the polyisocyanate, it can participate in both light and moisture curing, so that its strength is still high under no light conditions. The UV moisture dual-curing reactive polyurethane hot melt adhesive of the present invention has the characteristics of rapid bonding and fixing of UV glue, and high reliability of polyurethane hot melt adhesive, and has a high curing strength when cured under no light conditions. DETAILED DESCRIPTION
[0027] The principles and features of the present invention are described below in conjunction with examples. The examples are only used to explain the present invention and are not used to limit the scope of the present invention.
[0028] Embodiment 1:
[0029] Preparation of polyols with acrylates:
[0030] 1 mol of polycaprolactone triol 305T (Dacel (China) Investment Co., Ltd.) was pre-dehydrated at 100°C for 12 h and then cooled to 80°C. 1 mol of MOI and 0.01 g of phenothiazine were added to the reaction bottle and heated to 120°C. The reaction was continued for 90 min. The vacuum was broken with nitrogen and the mixture was poured into a sealed container to isolate the mixture from moisture and then used as prepolymer A-1.
[0031] Embodiment 2:
[0032] Preparation of polyols with acrylates:
[0033] 1 mol of polycaprolactone triol 305T (Dacel (China) Investment Co., Ltd.) was pre-dehydrated at 100°C for 12 h and then cooled to 80°C. 1.25 mol of MOI and 0.01 g of phenothiazine were added to the reaction bottle and heated to 120°C. The reaction was continued for 90 min. The vacuum was broken with nitrogen and the mixture was poured into a sealed container and kept away from moisture for later use. This was recorded as prepolymer A-2.
[0034] Embodiment 3:
[0035] Preparation of UV moisture dual curing reactive polyurethane hot melt adhesive:
[0036] Weigh 90g of Dynacoll 7360, 45g of Evonik Dynacoll 7255, 30g of PPG2000 in a reactor, 10g of acrylic resin BR113, 10g of petroleum resin, 90g of prepolymer A-1, dehydrate for 2h at 140℃ and reduced pressure of -0.095MPa, then lower the temperature to 100℃, add 70g of diphenylmethane-4,4'-diisocyanate (MDI), raise the temperature to 120℃ and continue to react for 45 minutes, then add 1g of mercaptopropyl trimethoxysilane, 0.6g of catalyst dimorpholinyl ethyl ether (DMDEE), 3.5g of photoinitiator TPO, and continue to react for 45 minutes. Then break the vacuum with nitrogen, fill it into a specific sealed container while hot, and wait for testing.
[0037] Embodiment 4:
[0038] Preparation of UV moisture dual curing reactive polyurethane hot melt adhesive:
[0039] Weigh 90g of Dynacoll 7360, 45g of Evonik Dynacoll 7255, 30g of PPG2000 in a reactor, 10g of acrylic resin BR113, 10g of petroleum resin, 90g of prepolymer A-2, dehydrate for 2h at 140℃ under reduced pressure of -0.095MPa, then lower the temperature to 100℃, add 67g of MDI, raise the temperature to 120℃ and continue to react for 45 minutes, then add 1g of mercaptopropyltrimethoxysilane, 0.6g of catalyst DMDEE, 3.5g of photoinitiator TPO, and continue to react for 45 minutes. Then break the vacuum with nitrogen, fill it into a specific sealed container while hot, and wait for testing.
[0040] Embodiment 5:
[0041] Preparation of UV moisture dual curing reactive polyurethane hot melt adhesive:
[0042] Weigh 90g of Dynacoll 7360, 45g of Evonik Dynacoll 7255, 30g of PPG2000 in a reactor, 10g of acrylic resin BR113, 10g of petroleum resin, 30g of prepolymer A-1, dehydrate for 2h at 140℃ under reduced pressure of -0.095MPa, then lower the temperature to 100℃, add 50g of MDI, raise the temperature to 120℃ and continue to react for 45 minutes, then add 1g of mercaptopropyltrimethoxysilane, 0.6g of catalyst DMDEE, 3.5g of photoinitiator TPO, and continue to react for 45 minutes. Then break the vacuum with nitrogen, fill into a specific sealed container while hot, and wait for testing.
[0043] Embodiment 6:
[0044] Preparation of UV moisture dual curing reactive polyurethane hot melt adhesive:
[0045] Weigh 90g of Dynacoll 7360, 45g of Evonik Dynacoll 7255, 30g of PPG2000 in a reactor, 10g of acrylic resin BR113, 10g of petroleum resin, 60g of prepolymer A-1, dehydrate for 2h at 140℃ and reduced pressure of -0.095MPa, then lower the temperature to 100℃, add 60g of MDI, raise the temperature to 120℃ and continue to react for 45 minutes, then add 1g of mercaptopropyltrimethoxysilane, 0.6g of catalyst DMDEE, 3.5g of photoinitiator TPO, and continue to react for 45 minutes. Then break the vacuum with nitrogen, fill it into a specific sealed container while hot, and wait for testing.
[0046] Comparative Example 1:
[0047] Weigh 90g of Dynacoll 7360, 45g of Evonik Dynacoll 7255, 30g of PPG2000 in a reactor, 70g of acrylic resin BR113, 10g of petroleum resin, dehydrate for 2h at 140℃ and reduced pressure of -0.095MPa, then lower the temperature to 100℃, add 40g of MDI, raise the temperature to 120℃ and continue to react for 45 minutes, then add 1g of mercaptopropyltrimethoxysilane, 0.6g of catalyst DMDEE, 3.5g of photoinitiator TPO, and continue to react for 45 minutes. Then break the vacuum with nitrogen, fill it into a specific sealed container while hot, and wait for testing.
[0048] The present invention needs to carry out the following performance tests:
[0049] 1. Samples, substrates and curing conditions
[0050] Selected substrate: PC + 20% GF;
[0051] Pull-out strength test: 3mm diameter dot;
[0052] Colloid thickness: 0.15mm;
[0053] Stretching speed: 10mm1min;
[0054] Curing conditions: 25°C, 50% humidity, curing for 1min, 5min, 24h;
[0055] UV light curing: 365nm (800mw*5s);
[0056] Test environment temperature: 25℃.
[0057] 2. Strength test
[0058] Light intensity: Apply a 3mm diameter glue dot to the substrate surface, add a 0.15mm gap sheet, press the second sheet, use a 1kg weight to press for 10s, irradiate with a UV lamp with a wavelength of 365nm for 5s, and then maintain the pressure for a fixed time.
[0059] No light intensity: Apply a 3mm diameter glue dot to the substrate surface, add a 0.15mm gap sheet, press the second sheet, use a 1kg weight to press for 10s, and then maintain the pressure for a fixed time.
[0060] The test results of the hot melt adhesives obtained in Examples 3-6 and Comparative Example 1 are shown in the following table:
[0061] Table 1 Test results of examples and comparative examples
[0062]
[0063]
[0064] It can be seen from the test results in Table 1 that the UV moisture dual-curing reactive polyurethane hot melt adhesive prepared by adding polyols with acrylates in the present invention has excellent initial and final bonding strengths; the un-illuminated area still has a high bonding strength (in the absence of light, the pull-out strength is 3-4MPa, which is already very high and sufficient to meet the application requirements); the UV moisture dual-curing reactive polyurethane hot melt adhesive prepared by adding polyols with acrylates in the present invention can participate in both light and moisture curing, so that it still has a high strength under no light conditions; it has the characteristics of rapid bonding and fixing of UV adhesives and high reliability of polyurethane hot melt adhesives. In addition, it can meet the needs of environmental protection, low odor, and rapid fixing and bonding in the field of electronic packaging.
[0065] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a UV moisture dual-curing reactive polyurethane hot melt adhesive, characterized in that: The steps include: Weigh 90g of Dynacoll 7360, 45g of Evonik Dynacoll 7255, 30g of PPG2000, 10g of acrylic resin BR113, 10g of petroleum resin, 90g of prepolymer A-2 in a reactor, dehydrate for 2h at 140°C under reduced pressure of -0.095MPa, then reduce the temperature to 100°C, add 67g of diphenylmethane-4,4'-diisocyanate MDI, heat to 120°C and continue to react for 45 minutes, then add 1g of mercaptopropyltrimethoxysilane, 0.6g of catalyst dimorpholinylethyl ether DMDEE, 3.5g of photoinitiator TPO, continue to react for 45 minutes, then break the vacuum, discharge the material, and seal and package to obtain a UV moisture dual-curing reactive polyurethane hot melt adhesive; The preparation method of the prepolymer A-2 comprises the following steps: Dehydrate 1 mol of polycaprolactone triol 305T at 100°C / 2h in advance, cool to 80°C, add 1.25 mol of isocyanoethyl methacrylate MOI and 0.01 g of phenothiazine into the reaction bottle, heat to 120°C, continue the reaction for 90 min, break the vacuum with nitrogen, pour into a sealed container, isolate from moisture and set aside.