A kind of polyaniline photothermal energy storage nanofiber and preparation method thereof

Through emulsion polymerization and electrospinning technology, the poor solubility and compatibility problems of polyaniline in the spinning liquid were solved, and polyaniline photothermal energy storage nanofibers with photothermal conversion and energy storage and temperature regulation were prepared to realize Efficient solar energy storage and conversion.

CN115852527BActive Publication Date: 2024-11-08ZHEJIANG SCI-TECH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211499438.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-28
Publication Date
2024-11-08
Estimated Expiration
2042-11-28

AI Technical Summary

Technical Problem

Polyaniline has poor solubility in spinning liquid and compatibility with phase change materials, making it difficult to be used in electrospinning to prepare photothermal energy storage nanofibers.

Method used

The O/W emulsion of polyaniline/phase change material was prepared by emulsion polymerization, and combined with polyvinyl alcohol. Polyaniline photothermal energy storage nanofibers were prepared by electrospinning technology, which solved the poor water solubility and compatibility of polyaniline. Sexual problems.

Benefits of technology

The preparation of polyaniline photothermal energy storage nanofibers is realized, with good photothermal conversion and energy storage and temperature adjustment functions, avoiding the poor water solubility of polyaniline, and improving compatibility with phase change materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115852527B_ABST
    Figure CN115852527B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for preparing polyaniline photothermal energy storage nanofibers, aiming to solve the problems of poor solubility of polyaniline in spinning solution and compatibility with phase change materials. A polyaniline photothermal energy storage nanofiber comprises a core layer for photothermal conversion and energy storage and temperature regulation, and a sheath layer covering the core layer; the core layer is a photothermal conversion material and an energy storage and temperature regulation material; the sheath layer is a polymer material. A method for preparing polyaniline photothermal energy storage nanofibers comprises the following steps: first preparing an O / W emulsion of polyaniline / phase change material; then preparing a spinning solution of polyaniline / phase change material / polyvinyl alcohol O / W emulsion; and finally preparing the polyaniline photothermal energy storage nanofibers by electrostatic spinning.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of photothermal energy storage, and in particular to polyaniline photothermal energy storage nanofibers and a preparation method thereof. Background Art

[0002] As one of the most abundant and cleanest renewable energy sources, the photothermal conversion application of solar energy has received widespread attention. The capture, conversion and storage of solar energy by photothermal energy storage is an effective way to utilize solar energy, and its ability is affected by the thermophysical properties of photothermal conversion materials and heat storage materials. Photothermal conversion materials are severely restricted by intermittent solar radiation when utilizing solar energy, and the converted thermal energy cannot be stored for a long time, while the latent heat of phase change materials can collect and store the thermal energy converted from solar energy. Therefore, combining photothermal conversion materials and phase change materials can collect, store and convert solar energy more efficiently, and the operation is simple and has great feasibility.

[0003] Phase change materials achieve energy storage and temperature regulation functions through reversible phase transitions, have high heat storage energy, and can be recycled indefinitely. Among them, aliphatic ester phase change materials have suitable phase change temperatures, high latent heat values, and cost-effectiveness, and have great application potential in the field of energy storage and heat storage. Polyaniline is a conductive polymer with good chemical stability and special optical properties. Its special conjugated structure (PANI) enables it to have a strong light absorption effect in the ultraviolet-visible-near infrared region, and it is a type of efficient semiconductor photothermal conversion material. There have been many reports on the research and application of aliphatic ester phase change materials in the field of electrospun temperature regulation and heat storage nanofibers, but there are few studies on the application of polyaniline in the field of electrospun photothermal energy storage nanofibers. The reason is that polyaniline has a relatively hard skeleton structure and a high degree of conjugation, making it difficult to dissolve in most solvents. In addition, polyaniline usually exists in the form of low molecular weight, which easily affects the viscosity of the solution, making it difficult to use polyaniline to prepare nanofibers by electrospinning. Therefore, solving the solubility problem of the photothermal conversion material polyaniline in the spinning solution, improving its compatibility with the phase change material, and establishing a method for preparing polyaniline photothermal energy storage composite nanofiber materials by electrospinning are technical problems that need to be solved at present. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing polyaniline photothermal energy storage nanofibers, aiming to solve the problems of poor solubility of polyaniline in spinning solution and compatibility with phase change materials.

[0005] To solve the above technical problems, the purpose of the present invention is achieved as follows:

[0006] A polyaniline photothermal energy storage nanofiber, comprising a core layer for photothermal conversion and energy storage temperature regulation, and a sheath layer covering the core layer;

[0007] The core layer is made of photothermal conversion material and energy storage and temperature regulation material; the sheath layer is made of polymer material.

[0008] On the basis of the above scheme and as a preferred scheme of the above scheme: the photothermal conversion material is polyaniline, which is formed by emulsion polymerization of aniline monomer; the energy storage temperature regulating material is a phase change material of fatty acid esters, which can be selected from one of lauryl dodecyl, tetradecyl myristate or hexadecyl palmitate phase change materials, wherein the phase change temperature is 25-50°C, and the latent heat value is ≥200J / g; the polymer material is polyvinyl alcohol, with a molecular weight of 110,000-130,000 and a degree of alcoholysis of 88%-98%.

[0009] A method for preparing polyaniline photothermal energy storage nanofibers comprises the following steps:

[0010] Firstly, an O / W emulsion of polyaniline / phase change material is prepared;

[0011] Then preparing a spinning solution of polyaniline / phase change material / polyvinyl alcohol O / W type emulsion;

[0012] Finally, polyaniline photothermal energy storage nanofibers were prepared by electrospinning.

[0013] On the basis of the above scheme and as a preferred scheme of the above scheme: the polyaniline / phase change material O / W emulsion further includes monomers, initiators, solvents, emulsifiers, dopants and pH regulators. The spinning solution also includes a crosslinking agent.

[0014] On the basis of the above scheme and as a preferred scheme of the above scheme: the pH value of the polyaniline / phase change material O / W emulsion is 4-5, and the pH value of the spinning solution is 4-5.

[0015] On the basis of the above scheme and as a preferred scheme of the above scheme: the preparation of the O / W emulsion of polyaniline / phase change material comprises the following steps:

[0016] (1) preparing an aqueous solution of a first type emulsifier, adding a phase change material to the aqueous solution of the first type emulsifier, stirring at 80° C. and 8000 r / min for 30 min, to obtain an O / W type emulsion of the phase change material;

[0017] (2) preparing an aqueous solution of a second type emulsifier, adding aniline to the aqueous solution of the second type emulsifier, stirring at 50° C. and 6000 r / min for 20 min, to obtain an O / W type emulsion of aniline;

[0018] (3) The O / W emulsion of phase change material and the O / W emulsion of aniline are cooled to 0-5° C., and then mixed under continuous stirring to form a composite emulsion of aniline / phase change material; 1M hydrochloric acid is added to the composite emulsion of aniline / phase change material, and stirred at 1000 r / min for 0.5 h in an ice-water bath, and then an aqueous solution of ammonium persulfate is added, and stirring is continued at 500 r / min for 10 h; after the reaction is completed, a small amount of 0.05M sodium hydroxide is added to the obtained emulsion, the pH value is adjusted to 4-5, and then the concentrated emulsion is filtered to obtain an O / W emulsion of polyaniline / phase change material.

[0019] On the basis of the above scheme and as a preferred scheme of the above scheme: the preparation of the spinning solution of polyaniline / phase change material / polyvinyl alcohol O / W type emulsion includes the following steps:

[0020] (1) Add polyvinyl alcohol to cold water and mix, transfer to a 250 ml three-necked flask, then heat to 90° C. in a constant temperature water bath, and stir at 200 r / min for 3 h to obtain a polyvinyl alcohol aqueous solution;

[0021] (2) Adding poly(vinyl alcohol) aqueous solution to polyaniline / phase change material O / W type emulsion, stirring at 80°C and 10000 r / min for 0.5 h, standing to cool to room temperature, adding a cross-linking agent, continuing to stir for 10 min, and eliminating bubbles by ultrasonication to obtain a spinning solution of polyaniline / phase change material / poly(vinyl alcohol) O / W type emulsion;

[0022] On the basis of the above scheme and as a preferred scheme of the above scheme: electrospinning comprises the following steps:

[0023] The spinning solution of polyaniline / phase change material / polyvinyl alcohol O / W type emulsion is added into the syringe of the electrospinning device, the spinning needle is a No. 21 needle, the spinning voltage is 18-22KV, the emulsion flow rate is 1-1.5mL / h, the receiving speed is 80-100rpm, the spinning distance is 12-18cm, the translation distance is 100mm, the spinning temperature and humidity are controlled at 25-30℃ and 50%-60% respectively, and electrospinning is carried out to collect polyaniline photothermal energy storage nanofibers.

[0024] On the basis of the above scheme and as a preferred scheme of the above scheme: the spinning solution of polyaniline photothermal energy storage nanofibers is mainly made of the following raw materials in terms of mass percentage: 9.1% to 13.7% of polymer materials, 3.6% to 6.0% of photothermal conversion materials, 4.5% to 6.8% of energy storage temperature regulating materials, 0.9% to 1.7% of emulsifiers and 71.9% to 81.8% of solvents, 0.3% to 0.5% of pH regulators and 0.7% to 1.1% of cross-linking agents.

[0025] On the basis of the above scheme and as a preferred scheme of the above scheme: the first emulsifier and the second emulsifier are sodium dodecyl sulfate and Tween-20 respectively; aniline is the polymerization monomer; ammonium persulfate is the initiator; hydrochloric acid is the oxidant and dopant; the solvent is deionized water; and sodium hydroxide is the pH regulator.

[0026] On the basis of the above scheme and as a preferred scheme of the above scheme: the cross-linking agent is glutaraldehyde and the solvent is deionized water.

[0027] On the basis of the above scheme and as a preferred scheme of the above scheme: the fiber diameter of the prepared aniline photothermal energy storage nanofibers is 400-800nm; the photothermal conversion efficiency is 60%-80.0%; the latent heat value is 40-65J / g; and the breaking strength is 10.0-18.0MPa.

[0028] The basic method and principle of the present invention are as follows: in the preparation of polyaniline by emulsion polymerization, since polyaniline is insoluble in water, the emulsion polymerization with aniline as the monomer is mainly based on micelle nucleation. The polyaniline produced by the polymerization reaction of aniline in the solubilized micelle of Tween-20 is insoluble in the solvent ion water, and it will enter and exit the O / W type emulsion system of the phase change material under the action of mechanical stirring, and finally form the O / W composite emulsion system of polyaniline / phase change material under the action of the emulsifier. Prepare a polyvinyl alcohol aqueous solution, mix the polyvinyl alcohol aqueous solution with the O / W composite emulsion of polyaniline / phase change material under high-speed stirring, and form a spinning solution of an O / W type emulsion with the polyvinyl alcohol aqueous solution as the water phase and polyaniline and the phase change material as the oil phase. Use glutaraldehyde to carry out in-situ crosslinking modification treatment on polyvinyl alcohol, and prepare polyaniline photothermal energy storage nanofibers by emulsion electrospinning technology.

[0029] In summary, the beneficial effects of the present invention are:

[0030] In order to obtain a nanofiber with both photothermal conversion and energy storage and temperature regulation functions, we used emulsion spinning technology to prepare a polyaniline photothermal energy storage composite nanofiber with good photothermal conversion and energy storage and temperature regulation functions, using photothermal conversion material and phase change material as the core layer and polymer material as the sheath layer.

[0031] We proposed a new polyaniline synthesis scheme, in which polyaniline was synthesized by emulsion polymerization in a system of a mixture of an O / W emulsion of a phase change material and an O / W emulsion of aniline, and an O / W composite emulsion of polyaniline / phase change material was formed, and then combined with a polymer solution, polyaniline photothermal energy storage composite nanofibers were prepared by emulsion electrospinning technology. This scheme avoids the disadvantage of poor water solubility of polyaniline and solves the compatibility problem of combining polyaniline with phase change materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 This is a scanning electron microscope image of a polyaniline photothermal energy storage nanofiber according to an embodiment of the present application.

[0033] Figure 2 This is a latent heat value diagram of a polyaniline photothermal energy storage nanofiber according to an embodiment of the present application.

[0034] Figure 3 This is a schematic diagram of the change in film surface temperature of a polyaniline photothermal energy storage nanofiber under the sun over time in an embodiment of the present application, wherein the arrow indicates the start time of illumination.

[0035] Figure 4 It is a stress-strain schematic diagram of a polyaniline photothermal energy storage nanofiber according to an embodiment of the present application.

[0036] Figure 5 These are pictures of an O / W type emulsion of polyaniline / phase change material of an embodiment of the present application before and after being stationary for 1 week. DETAILED DESCRIPTION

[0037] The preparation of the polyaniline photothermal energy storage nanofibers of the present invention is described in detail below through specific examples; in the following examples, unless otherwise specified, the reagents, materials and equipment used can be purchased from commercial sources, or prepared by conventional methods, or commonly used in the industry. Unless otherwise specified, all percentages are in mass units. The examples cited are only used to explain the present invention and are not used to limit the scope of the present invention.

[0038] Example 1

[0039] Preparation of polyaniline photothermal energy storage nanofibers:

[0040] (1) preparing 50.0 ml of an aqueous solution of 0.4 g of sodium dodecyl sulfate; adding 5.0 g of dodecyl laurate to the aqueous emulsifier solution, and emulsifying at 80° C. and 8000 r / min for 30 min to obtain an O / W emulsion of dodecyl laurate;

[0041] (2) preparing 50.0 ml of an aqueous solution of 0.6 g of Tween-20; adding 5.0 g of aniline to the aqueous emulsifier solution, and emulsifying at 50° C. and 6000 r / min for 20 min to obtain an O / W emulsion of aniline;

[0042] (3) cooling the O / W type emulsion of lauryl laurate and the O / W type emulsion of aniline to a temperature of 0 to 5° C., and mixing them under continuous stirring to form an aniline / lauryl laurate composite emulsion;

[0043] (4) Add 100.0 g of 1 M hydrochloric acid to the composite emulsion of aniline / dodecanoate, stir at 1000 r / min for 0.5 h using a constant speed electric stirrer in an ice water bath, then add 6.13 g of ammonium persulfate in 10.0 ml of an aqueous solution, continue magnetic stirring at 500 r / min, and polymerize for 10 h; after the reaction is completed, drop a small amount of 0.05 M sodium hydroxide into the obtained emulsion, adjust the pH value to 4-5, and then filter and concentrate the emulsion to obtain an O / W type emulsion of polyaniline / dodecanoate.

[0044] (5) 20.0 g of polyvinyl alcohol was added to 80% cold water and mixed, and the mixture was transferred to a 250 ml three-necked flask. The three-necked flask was then fixed in a constant temperature water bath and heated to 90° C. The mixture was stirred at a speed of 200 r / min for 3 h using a constant speed electric stirrer to obtain a polyvinyl alcohol aqueous solution;

[0045] (6) adding 50.0 g of polyaniline / dodecanoate O / W type emulsion to 60.0 g of polyaniline / dodecanoate O / W type emulsion, stirring at a constant temperature of 70° C. with a constant speed electric stirrer at a speed of 10000 r / min for 0.5 h, standing to cool to room temperature, adding 0.8 g of glutaraldehyde, continuing to stir for 10 min, and eliminating bubbles by ultrasound until the mixed solution is uniformly dispersed; obtaining a spinning solution of polyaniline / dodecanoate / polyvinyl alcohol O / W type emulsion;

[0046] (7) The polymer spinning solution was added into the syringe of the electrospinning device. The spinning needle was a No. 21 needle. The spinning voltage was 18 KV, the emulsion flow rate was 1 mL / h, the receiving speed was 80 rpm, the spinning distance was 18 cm, the translation distance was 100 mm, and the spinning temperature and humidity were controlled at 30 ° C and 50% respectively. Electrospinning was performed to collect polyaniline photothermal energy storage nanofibers.

[0047] Example 2

[0048] Preparation of a polyaniline photothermal energy storage nanofiber:

[0049] The difference between this embodiment and Example 1 is that the amount of raw material added to the polymer spinning solution is different, the amount of polyvinyl alcohol added is 22.4 g, the electrospinning parameters are different, the spinning voltage is 20 KV, and the emulsion flow rate is 1.2 mL / h.

[0050] Example 3

[0051] Preparation of a polyaniline photothermal energy storage nanofiber:

[0052] The difference between it and Example 1 is that the amount of raw material added to the polymer spinning solution is different, and the amount of polyvinyl alcohol added is 25.6 g. The electrospinning parameters are different, the spinning voltage is 22 KV, the emulsion flow rate is 1.0 mL / h, the receiving speed is 100 rpm, and the spinning temperature and humidity are controlled at 25° C. and 60%, respectively.

[0053] Example 4

[0054] Preparation of a polyaniline photothermal energy storage nanofiber:

[0055] (1) preparing 80.0 ml of an aqueous solution of 0.8 g of sodium dodecyl sulfate; adding 8.0 g of dodecyl laurate to the aqueous emulsifier solution, and emulsifying at 80° C. and 8000 r / min for 30 min to obtain an O / W emulsion of dodecyl laurate;

[0056] (2) preparing 70.0 ml of an aqueous solution of 1.2 g of Tween-20; adding 7.0 g of aniline to the aqueous emulsifier solution, and emulsifying at 50° C. and 6000 r / min for 20 min to obtain an O / W emulsion of aniline;

[0057] (3) cooling the O / W type emulsion of lauryl laurate and the O / W type emulsion of aniline to a temperature of 0 to 5° C., and mixing them under continuous stirring to form an aniline / lauryl laurate composite emulsion;

[0058] (4) Add 150.0g of 1M hydrochloric acid to the composite emulsion of aniline / dodecanoic acid ester, stir at 1000r / min for 0.5h using a constant speed electric stirrer under ice water bath conditions, then add 8.58g of ammonium persulfate in 10.0ml of aqueous solution, continue magnetic stirring at 500r / min, and the polymerization time is 10h. After the reaction is completed, drop a small amount of 0.05M sodium hydroxide into the obtained emulsion, adjust the pH value to 4-5, and then filter and concentrate the emulsion to obtain an O / W type emulsion of polyaniline / dodecanoic acid ester.

[0059] (5) 22.4 g of polyvinyl alcohol was added to 80% cold water and mixed, and the mixture was transferred to a 250 ml three-necked flask. The three-necked flask was then fixed in a constant temperature water bath and heated to 90° C. The mixture was stirred at a speed of 200 r / min for 3 h using a constant speed electric stirrer to obtain a polyvinyl alcohol aqueous solution;

[0060] (6) adding 50.0 g of polyaniline / dodecanoate O / W type emulsion to 60.0 g of polyaniline / dodecanoate O / W type emulsion, stirring at a constant temperature of 70° C. with a constant speed electric stirrer at a speed of 10000 r / min for 0.5 h, standing to cool to room temperature, adding 0.8 g of glutaraldehyde, continuing to stir for 10 min, and eliminating bubbles by ultrasound until the mixed solution is uniformly dispersed; obtaining a spinning solution of polyaniline / dodecanoate / polyvinyl alcohol O / W type emulsion;

[0061] (7) The polymer spinning solution was added into the syringe of the electrospinning device. The spinning needle was a No. 21 needle. The spinning voltage was 20 KV, the emulsion flow rate was 1.2 mL / h, the receiving speed was 80 rpm, the spinning distance was 18 cm, the translation distance was 100 mm, and the spinning temperature and humidity were controlled at 30 ° C and 50% respectively. Electrospinning was performed to collect polyaniline photothermal energy storage nanofibers.

[0062] Example 5

[0063] Preparation of a polyaniline photothermal energy storage nanofiber:

[0064] (1) preparing 70.0 ml of an aqueous solution of 0.6 g of sodium dodecyl sulfate; adding 7.0 g of dodecyl laurate to the aqueous emulsifier solution, and emulsifying at 80° C. and 8000 r / min for 30 min to obtain an O / W emulsion of dodecyl laurate;

[0065] (2) preparing 60.0 ml of an aqueous solution of 1.0 g of Tween-20; adding 6.0 g of aniline to the aqueous emulsifier solution, and emulsifying at 50° C. and 6000 r / min for 20 min to obtain an O / W emulsion of aniline;

[0066] (3) cooling the O / W type emulsion of lauryl laurate and the O / W type emulsion of aniline to a temperature of 0 to 5° C., and mixing them under continuous stirring to form an aniline / lauryl laurate composite emulsion;

[0067] (4) Add 130.0g of 1M hydrochloric acid to the composite emulsion of aniline / dodecanoic acid ester, stir at 1000r / min for 0.5h using a constant speed electric stirrer under ice water bath conditions, then add 7.35g of ammonium persulfate in 10.0ml of aqueous solution, continue magnetic stirring at 500r / min, and the polymerization time is 10h. After the reaction is completed, drop a small amount of 0.05M sodium hydroxide into the obtained emulsion, adjust the pH value to 4-5, and then filter and concentrate the emulsion to obtain an O / W type emulsion of polyaniline / dodecanoic acid ester.

[0068] Its steps (5), (6) and (7) are the same as those in Example 4.

[0069] Example 6

[0070] Preparation of a polyaniline photothermal energy storage nanofiber:

[0071] (1) preparing 60.0 ml of an aqueous solution of 0.5 g of sodium dodecyl sulfate; adding 6.0 g of dodecyl laurate to the aqueous emulsifier solution, and emulsifying at 80° C. and 8000 r / min for 30 min to obtain an O / W type emulsion of dodecyl laurate;

[0072] (2) preparing 50.0 ml of an aqueous solution of 0.8 g of Tween-20; adding 5.0 g of aniline to the aqueous emulsifier solution, and emulsifying at 50° C. and 6000 r / min for 20 min to obtain an O / W emulsion of aniline;

[0073] (3) cooling the O / W type emulsion of lauryl laurate and the O / W type emulsion of aniline to a temperature of 0 to 5° C., and mixing them under continuous stirring to form an aniline / lauryl laurate composite emulsion;

[0074] (4) Add 110.0g of 1M hydrochloric acid to the composite emulsion of aniline / dodecanoic acid ester, stir at 1000r / min for 0.5h using a constant speed electric stirrer under ice water bath conditions, then add 6.13g of ammonium persulfate in 10.0ml of aqueous solution, continue magnetic stirring at 500r / min, and the polymerization time is 10h. After the reaction is completed, drop a small amount of 0.05M sodium hydroxide into the obtained emulsion, adjust the pH value to 4-5, and then filter and concentrate the emulsion to obtain an O / W type emulsion of polyaniline / dodecanoic acid ester.

[0075] Its steps (5), (6) and (7) are the same as those in Example 4.

[0076] Comparative Example

[0077] A method for preparing polyvinyl alcohol nanofibers:

[0078] (1) 14 g of polyvinyl alcohol was added to 86.0 g of cold water, and the mixture was transferred to a 250 ml three-necked flask. The three-necked flask was then fixed in a constant temperature water bath and heated to 90° C. The mixture was stirred at a speed of 200 r / min for 3 h using a constant speed electric stirrer to obtain a polyvinyl alcohol spinning solution.

[0079] (2) The polyvinyl alcohol spinning solution was added into the syringe of the electrospinning device. The spinning needle was a No. 21 needle. The spinning voltage was 20 KV, the emulsion flow rate was 1.2 mL / h, the receiving speed was 80 rpm, the spinning distance was 18 cm, the translation distance was 100 mm, and the spinning temperature and humidity were controlled at 30°C and 50%, respectively, to perform electrospinning to collect polyvinyl alcohol nanofibers.

[0080] Performance testing

[0081] (1) Surface morphology observation

[0082] The polyaniline photothermal energy storage nanofibers obtained in Example 4 were taken as samples, and the microstructure of the samples was observed using a scanning electron microscope.

[0083] (2) Latent heat value test

[0084] The polyaniline photothermal energy storage nanofibers obtained in Example 4 were taken as samples, and the latent heat value of the samples was detected using a photocalorimetric differential scanning calorimeter.

[0085] (3) Characterization of photothermal conversion performance

[0086] The polyaniline photothermal energy storage nanofiber obtained in Example 4 was taken as a sample, and the surface temperature change of the sample under one sun with time was recorded by a temperature recorder sensor.

[0087] (3) Mechanical properties test

[0088] The polyaniline photothermal energy storage nanofibers obtained in Example 4 were taken as samples, and the stress-strain mechanical properties of the samples were tested using a uniaxial tensile instrument.

[0089] In the description of the present invention, it should be understood that the terms "upper", "lower", "top", "bottom", "inside", "outside", etc. indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, or are the orientations or positional relationships in which the inventive product is conventionally placed when in use, or are the orientations or positional relationships conventionally understood by those skilled in the art. They are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.

[0090] In addition, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. In the present invention, unless otherwise clearly specified and limited, the terms "install", "set", "connect", "fix", "screw" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral one; it can be a mechanical connection or an electrical connection;

[0091] The above embodiments are only preferred embodiments of the present invention and are not intended to limit the protection scope of the present invention. Therefore, any equivalent changes made based on the structure, shape, and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing polyaniline photothermal energy storage nanofibers, characterized in that: The polyaniline photothermal energy storage nanofiber contains a core layer for photothermal conversion and energy storage and temperature regulation, and a sheath layer covering the core layer; the core layer is a photothermal conversion material and an energy storage and temperature regulation material; the sheath layer is a polymer material; The photothermal conversion material is polyaniline, which is formed by emulsion polymerization of aniline monomer; the energy storage temperature regulating material is a phase change material of fatty acid esters, which is selected from one of lauryl laurate, tetradecyl myristate or hexadecyl palmitate phase change materials, wherein the phase change temperature is 25-50°C, and the latent heat value is ≥200J / g; the polymer material is polyvinyl alcohol, which is selected from a molecular weight of 110,000-130,000 and an alcoholysis degree of 88%-98%; The steps include: Firstly, an O / W emulsion of polyaniline / phase change material is prepared; The following steps are included: (1) preparing an aqueous solution of a first type emulsifier, adding a phase change material to the aqueous solution of the first type emulsifier, stirring at 80° C. and 8000 r / min for 30 min, to obtain an O / W type emulsion of the phase change material; (2) preparing an aqueous solution of a second type emulsifier, adding aniline to the aqueous solution of the second type emulsifier, stirring at 50° C. and 6000 r / min for 20 min, to obtain an O / W type emulsion of aniline; (3) cooling the O / W emulsion of phase change material and the O / W emulsion of aniline to 0-5° C., and then mixing them under continuous stirring to form a composite emulsion of aniline / phase change material; then adding 1M hydrochloric acid to the composite emulsion of aniline / phase change material, stirring at 1000 r / min for 0.5 h in an ice-water bath, and then adding an aqueous solution of ammonium persulfate, and continuing to stir at 500 r / min for 10 h; after the reaction is completed, dropping a trace amount of 0.05M sodium hydroxide into the obtained emulsion, adjusting the pH value to 4-5, and then filtering and concentrating the emulsion to obtain an O / W emulsion of polyaniline / phase change material; A polyvinyl alcohol aqueous solution was prepared, and the polyvinyl alcohol aqueous solution was mixed with an O / W composite emulsion of polyaniline / phase change material under high-speed stirring to form a spinning solution of an O / W type emulsion with the polyvinyl alcohol aqueous solution as the water phase and polyaniline and the phase change material as the oil phase. The polyvinyl alcohol was subjected to in-situ cross-linking modification treatment using glutaraldehyde, and polyaniline photothermal energy storage nanofibers were prepared by emulsion electrospinning technology.

2. The method for preparing polyaniline photothermal energy storage nanofibers according to claim 1, characterized in that: The preparation of the spinning solution of an O / W type emulsion with a polyvinyl alcohol aqueous solution as the water phase and polyaniline and a phase change material as the oil phase comprises the following steps: (1) Add polyvinyl alcohol to cold water and mix, transfer to a 250 ml three-necked flask, then heat to 90° C. in a constant temperature water bath, and stir at 200 r / min for 3 h to obtain a polyvinyl alcohol aqueous solution; (2) Adding polyvinyl alcohol aqueous solution to polyaniline / phase change material O / W type emulsion, stirring at 80°C and 10000 r / min for 0.5 h, standing to cool to room temperature, adding glutaraldehyde, continuing to stir for 10 min, and eliminating bubbles by ultrasound to obtain a spinning solution of O / W type emulsion with polyvinyl alcohol aqueous solution as water phase and polyaniline and phase change material as oil phase.

3. The method for preparing polyaniline photothermal energy storage nanofibers according to claim 1, characterized in that: Electrospinning, The following steps are included: The spinning solution of O / W type emulsion with polyvinyl alcohol aqueous solution as water phase and polyaniline and phase change material as oil phase was added into the syringe of electrospinning device. The spinning needle was No. 21 needle. The spinning voltage was 18-22KV, the emulsion flow rate was 1-1.5mL / h, the receiving speed was 80-100rpm, the spinning distance was 12-18cm, the translation distance was 100mm, and the spinning temperature and humidity were controlled at 25-30℃ and 50%-60% respectively to collect polyaniline photothermal energy storage nanofibers.

4. The method for preparing polyaniline photothermal energy storage nanofibers according to claim 1, characterized in that: Calculated by mass percentage, the spinning solution of polyaniline photothermal energy storage nanofibers is mainly made of the following raw materials: polymer material 9.1%~13.7%, photothermal conversion material 3.6%~6.0%, energy storage temperature regulating material 4.5%~6.8%, emulsifier 0.9%~1.7% and water 71.9%~81.8%.

5. The method for preparing polyaniline photothermal energy storage nanofibers according to claim 1, characterized in that: The first type emulsifier and the second type emulsifier are sodium dodecyl sulfate and Tween-20 respectively; aniline is the polymerization monomer; ammonium persulfate is the initiator; hydrochloric acid is the oxidant and dopant; sodium hydroxide is the pH regulator.

6. The method for preparing polyaniline photothermal energy storage nanofibers according to claim 1, characterized in that: The fiber diameter of the prepared aniline photothermal energy storage nanofibers is 400~800nm; the photothermal conversion efficiency is 60%~80.0%; the latent heat value is 40~65J / g; and the breaking strength is 10.0~18.0MPa.