A method for recovering lithium from a lithium-containing solution

By adjusting the pH value of the lithium-containing solution and mixing it with the metaaluminate solution, lithium adsorbent is generated, and through evaporation concentration and carbonate reaction, efficient separation and recovery of lithium elements is achieved, and lithium element recovery in the prior art is solved The problems of low efficiency and low resource recovery rate simplify the process flow and reduce energy consumption.

CN115872421BActive Publication Date: 2024-11-19BYD CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111163658.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-09-30
Publication Date
2024-11-19
Estimated Expiration
2041-09-30

AI Technical Summary

Technical Problem

In the preparation process of lithium carbonate, the recovery efficiency of lithium elements is low, and the separation effect of Na+ and K+ is poor, resulting in low resource recovery rate, long process cycle and high energy consumption.

Method used

By adjusting the pH value of the lithium-containing solution and mixing it with the metaaluminate solution, precipitation is used to form a lithium adsorbent, and the efficient separation and recovery of lithium elements can be achieved through evaporation concentration and carbonate reaction, while preparing recyclable lithium adsorbents .

Benefits of technology

It improves the recovery rate of lithium elements and the comprehensive recovery rate of resources, simplifies the process flow, reduces energy consumption, and is environmentally friendly in the process, suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115872421B_ABST
    Figure CN115872421B_ABST
Patent Text Reader

Abstract

The present application provides a method for recovering lithium from a lithium-containing solution, wherein the lithium-containing solution with or without pH adjustment is mixed with aluminate, and the pH value is adjusted to weak acidity / neutral, so that the lithium element in the lithium-containing solution can be recovered as Li a X·2Al(OH)3·nH2O is separated from the system in the form of a precipitate, which is then converted into a lithium adsorbent (1‑m)Li a X·2Al(OH)3·nH2O and Li a X filtrate, and finally Li a The X filtrate is reacted with lithium to produce high-purity Li2CO3. This method achieves efficient separation of lithium elements and impurity ions, and produces a recyclable lithium adsorbent while recovering lithium, which can further recover the lithium-containing solution and has a high recovery rate of lithium in the lithium-containing solution. This method is simple in process, low in energy consumption, and environmentally friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the fields of environmental protection and resource recycling, and in particular to a method for recovering lithium from a lithium-containing solution. Background Art

[0002] Lithium carbonate is the basic material for the preparation of various industrial lithium salts. In the preparation process of lithium carbonate, due to its certain water solubility, a large amount of Li + And a certain amount of Na + and K + The industry generally removes Na from lithium-containing solutions by drying them in the sun or by strong evaporation. + and K + , and then adsorption, analysis and membrane concentration treatment are performed to recover lithium. The above method of recovering lithium has a long cycle and is + and K + The separation effect is poor and the recovery rate of lithium is low. Summary of the invention

[0003] In view of this, the present application provides a method for recovering lithium from a lithium-containing solution, which realizes the efficient separation of lithium elements and impurity ions, and produces a recyclable lithium adsorbent while recovering lithium, which can realize further recovery of the lithium-containing solution, has a high recovery rate of lithium in the lithium-containing solution, a high comprehensive recovery rate of resources, and the method has a simple process, low energy consumption, and is environmentally friendly.

[0004] Specifically, the present application provides a method for recovering lithium from a lithium-containing solution, comprising the following steps:

[0005] (1) Precipitating the lithium element in the lithium-containing solution by the following method a) or b):

[0006] a) adjusting the pH of the lithium-containing solution to 5-6 and then mixing it with the aluminate solution, allowing it to stand for aging to obtain a precipitate containing the first precipitate of Li(OH)·2Al(OH)3·nH2O, wherein n=1-3;

[0007] The pH value of the precipitate is adjusted to 6-7, and then filtered and washed to obtain Li a X·2Al(OH)3·nH2O precipitate and first filtrate;

[0008] b) Mixing the lithium-containing solution with the aluminate solution and adjusting the pH of the system to 5-7, allowing the reaction to stand for aging, filtering and precipitating to obtain Li a X·2Al(OH)3·nH2O precipitate and first filtrate;

[0009] Wherein, X represents the anion of the acid solution used to adjust the pH, and a=1 or 2;

[0010] (2) Lithium removal: a X·2Al(OH)3·nH2O precipitate was added to water and stirred for reaction, and the lithium adsorbent (1-m)Li was obtained by filtration. a X·2Al(OH)3·nH2O and Li a X filtrate, wherein m = 0.1-0.9;

[0011] (3) Lithium precipitation: a The X filtrate is evaporated and concentrated, carbonate is added for stirring reaction, and Li2CO3 precipitate is obtained after filtering and washing.

[0012] In the embodiment of the present application, the lithium-containing solution contains a large amount of Li + and CO3 2- 、Na + and K + Alkaline solutions containing impurity ions such as lithium precipitation mother liquor produced in the process of lithium extraction from salt lakes.

[0013] In method a), the pH value of the lithium-containing solution system is adjusted to 5-6 by adding an acid solution, so that the carbonate ions in the lithium-containing solution generate carbon dioxide and escape, thereby removing the carbonate ions in the system. It should be noted that the pH value of the lithium-containing solution system must be stabilized between 5-6 and no bubbles are generated, ensuring that there are no carbonate ions remaining in the system, before it is mixed with the aluminate solution to precipitate aluminum salts. In this process, the Li + It reacts with aluminate to form the first precipitate of Li(OH)·2Al(OH)3·nH2O. + Precipitate from lithium-containing solutions.

[0014] Preferably, the lithium-containing solution is stirred at a rate of 100 rpm to 500 rpm. A suitable stirring rate is beneficial to promoting the reaction between carbonate ions in the solution system and hydrogen ions in the acid solution.

[0015] The Li(OH)·2Al(OH)3·nH2O precipitate can be converted into Li(OH)·2Al(OH)3·nH2O by adding an acid solution to the precipitate solution containing the first precipitate of Li(OH)·2Al(OH)3·nH2O to adjust the pH value of the system to 6-7. a X·2Al(OH)3·nH2O precipitation to more efficiently carry out the subsequent lithium removal reaction and generate a lithium adsorbent with stronger adsorption capacity (1-m)Li a X·2Al(OH)3·nH2O, wherein X represents the anion of the acid solution used to adjust the pH, and a=1 or 2. X and a can be determined according to the type of the acid solution used to adjust the pH.

[0016] Wherein, in step (1), the acid solution used to adjust the pH may be one of sulfuric acid, hydrochloric acid, nitric acid or acetic acid. The type of acid solution is selected according to the type of anions in the lithium-containing solution, that is, for a chloride-type lithium-containing solution, the acid solution is hydrochloric acid; for a sulfate-type lithium-containing solution, the acid solution is sulfuric acid; for a nitrate-type lithium-containing solution, the acid solution is nitric acid; for an acetate-type lithium-containing solution, the acid solution is acetic acid. This can avoid the introduction of additional impurity ions into the system. When the acid solution used for pH is hydrochloric acid, X is Cl - When the acid solution is nitric acid, X is NO3 - When the acid solution is acetic acid, X is CH3COO - In the above three cases, a = 1. When the acid solution is sulfuric acid, X is SO4 2- , a=2.

[0017] Preferably, when the precipitate is stirred, the stirring rate is 100 rpm-300 rpm. Further preferably, after adjusting the pH value of the system to 6-7, stirring is continued for 0.5 h-1 h. Appropriate stirring rate and stirring time can promote the complete conversion of Li(OH)·2Al(OH)3·nH2O.

[0018] In method b), the aluminate solution is directly mixed with the lithium-containing solution, and then the pH value of the system is adjusted to 5-7 by an acid solution to directly obtain Li a X·2Al(OH)3·nH2O precipitation and first filtrate. It should be noted that Li a During the precipitation of X·2Al(OH)3·nH2O, carbonate ions in the system will also be removed by reacting to generate carbon dioxide. To ensure that there are no carbonate ions remaining in the system, filtration is performed only after no bubbles are generated in the system.

[0019] Preferably, the mixed solution of the metaaluminate solution and the lithium-containing solution obtained in the above method b) is stirred at a stirring rate of 100 rpm to 500 rpm. An appropriate stirring rate can allow the reactants to react completely.

[0020] Preferably, in both the method a) and the method b), the system can be subjected to ultrasound during the reaction between the acid solution and the carbonate ions. Ultrasound can effectively remove carbon dioxide bubbles generated by the reaction between the carbonate ions and the acid solution in the above system.

[0021] Preferably, the acid solution used in the method a) for adjusting the pH value of the lithium-containing solution and the acid solution used in the method b) are prepared by mixing one of commercially available concentrated hydrochloric acid (37 wt.%), commercially available concentrated sulfuric acid (98 wt.%), commercially available acetic acid (99.5 wt.%) or commercially available concentrated nitric acid (68 wt.%) with water in a mass ratio of (1-10):1; the acid solution used in the method a) for adjusting the pH value of the precipitation solution is an acid solution with a concentration of 2 wt.%-20 wt.%. An acid solution of appropriate concentration is conducive to the full reaction of the reactants.

[0022] In the present application, in order to avoid the introduction of additional impurity ions, the aluminate solution is generally sodium aluminate, potassium aluminate or ammonium aluminate. Preferably, the aluminate solution has a mass concentration of 4wt.%-16wt.%. Aluminate solution with an appropriate concentration is beneficial to ensure that Li + The rate of the precipitation reaction.

[0023] In some embodiments of the present application, aluminate is first mixed with water, and dissolved by stirring at 25°C-90°C, with a stirring rate of 100rpm-500rpm and a time of 0.5h-3h, until the solution is clear and transparent and the aluminate is completely dissolved.

[0024] In the embodiment of the present application, the lithium-containing solution and the aluminate are mixed at a molar ratio of Li:Al of (1.05-1.3):2. Mixing the aluminate with an excess of the lithium-containing solution can ensure that the aluminate reacts completely and no aluminum element remains in the system after the reaction.

[0025] Preferably, the aluminate solution and the lithium-containing solution can be mixed in three ways, specifically including: 1) adding the lithium-containing solution to the aluminate solution using a peristaltic pump, 2) adding the aluminate solution to the lithium-containing solution using a peristaltic pump, and 3) mixing the lithium-containing solution and the aluminate solution in parallel.

[0026] Preferably, in mode 1), the flow rate of the lithium-containing solution is 20 mL / min-5000 mL / min; in mode 2), the flow rate of the aluminate solution is 20 mL / min-5000 mL / min; in mode 3), the flow rates of the lithium-containing solution and the aluminate solution are both 20 mL / min-5000 mL / min. The specific liquid flow rate is calculated according to the concentrations of the aluminate solution and the lithium-containing solution in actual production conditions, and the molar ratio of Li to Al.

[0027] Further preferably, after the lithium-containing solution and the aluminate solution are mixed, the mixed solution of the two is stirred at a stirring rate of 100 rpm-500 rpm and a stirring time of 0.5 h-1 h. After the two are completely mixed, an acid solution is added to adjust the pH of the system.

[0028] In the embodiment of the present application, the time of the static aging described in step (1) is 1h-24h, and the temperature is 5°C-30°C. The static aging is to make the reactants (mainly including Li + and AlO2 - ) is fully reacted, and the generated suspension is allowed to settle, promoting the dissolution of small particles and the growth of large particles, so that the Li(OH)·2Al(OH)3·nH2O precipitation described in method a) or the Li(OH)·2Al(OH)3·nH2O precipitation described in method b) is obtained. a The particle size of the X·2Al(OH)3·nH2O precipitate is more uniform, which is more conducive to subsequent filtering and washing operations. The appropriate aging temperature can ensure that the above precipitate will not have the problem of lithium element escaping and causing its structure to be destroyed.

[0029] In the embodiment of the present application, step (1) further comprises: when adjusting the pH, collecting the carbon dioxide generated by the lithium-containing solution and passing it into an alkaline solution to obtain a carbonate; wherein the alkaline solution is NaOH or KOH, and the carbonate is Na2CO3 or K2CO3. In this way, resources can be fully utilized, the comprehensive recovery rate of resources can be improved, and production costs can be reduced. At the same time, the selection of NaOH or KOH also avoids the introduction of additional impurity ions. Preferably, the concentration of the alkaline solution is 4wt.%-15wt.%. The appropriate alkaline solution concentration can ensure the reaction rate of carbon dioxide.

[0030] In some embodiments of the present application, the CO2 generated by the reaction in step (1) is first introduced into a buffer storage tank, and an equal amount of alkali solution of equal concentration is introduced into sealed reactors No. 1 and No. 2, and then the CO2 in the buffer storage tank is introduced into sealed reactor No. 1, and the mass ratio of the amount of CO2 introduced to the alkali solution in sealed reactor No. 1 is (1.1-1.3): 1. When the pressure of the sealed reactor remains unchanged, the solution in sealed reactor No. 1 is transferred into sealed reactor No. 2, and the reaction is stirred for 0.5h-3h, and the stirring rate is 100rpm-500rpm. Finally, a carbonate solution for lithium precipitation is obtained.

[0031] In step (2), Li a The X·2Al(OH)3·nH2O precipitate is mixed with water to convert Li a The lithium element in X·2Al(OH)3·nH2O is partially extracted to prepare (1-m)Li a X·2Al(OH)3·nH2O, a lithium adsorbent with better lithium adsorption capacity, and Li-containing lithium carbonate for the subsequent step of preparing lithium carbonate a X filtrate.

[0032] Specifically, the reaction that occurs during the delithiation process is:

[0033]

[0034] The reverse reaction of the above reaction is the process in which the lithium adsorbent adsorbs lithium.

[0035] In the implementation mode of the present application, Li a The X·2Al(OH)3·nH2O precipitate is mixed with water at a mass ratio of 1:(1-50) and stirred at 20℃-60℃ for 1h-24h. By controlling the temperature and reaction time, the above reaction is promoted to the right, and the lithium adsorbent and Li-containing a The yield of the filtrate X. The adsorption and recovery of lithium element by the pathway described in the above reaction can improve the efficiency of lithium element adsorption and subsequent removal, thereby improving the recovery rate of lithium element.

[0036] In the present application, it is only necessary to introduce aluminate into the lithium-containing solution and adjust the pH to simultaneously obtain the recyclable lithium absorbing agent (1-m)Li during the recovery of lithium elements. a X·2Al(OH)3·nH2O has a simple preparation process and low cost.

[0037] In the embodiment of the present application, the lithium adsorbent (1-m)Li a The D50 particle size of X·2Al(OH)3·nH2O is 20μm-100μm, and the particle size range is 5μm-300μm. The appropriate particle size can ensure the adsorption efficiency of the lithium adsorbent.

[0038] Step (3) is to complete the precipitation of lithium element. a The X filtrate is evaporated and concentrated, and then carbonate is added for stirring reaction to convert lithium element into lithium carbonate precipitate, which is then filtered and washed to obtain Li2CO3 precipitate. Step (3) also includes drying the Li2CO3 precipitate at a temperature of 90°C-150°C for 2h-3h.

[0039] In the embodiment of the present application, the Li-containing a The X filtrate was evaporated and concentrated to a lithium concentration of 15g / L-25g / L. a The X filtrate was evaporated and concentrated, which increased the Li + The concentration is conducive to the subsequent lithium precipitation reaction and the precipitation of Li2CO3, and at the same time makes the subsequent filtration process easier to operate.

[0040] In the embodiment of the present application, the carbonate is added to the Li-containing aPreferably, the stirring rate is 100 rpm-500 rpm, and the carbonate solution is stirred for 0.5 h-1 h after addition, and then allowed to stand for 1 h-5 h to ensure that Li + The reaction is complete. Because lithium carbonate is slightly soluble in water, and the higher the temperature, the lower the solubility of lithium carbonate in water, so the temperature of the system should be maintained at 50℃-90℃, which is conducive to the precipitation of lithium carbonate from the solution, thereby increasing the reaction degree of lithium element in the system.

[0041] Preferably, the Li-containing a The molar ratio of Li element in the X filtrate to carbonate in the carbonate is (1.05-1.3):2. Wherein, the carbonate solution is a sodium carbonate solution or a potassium carbonate solution, and its concentration is 5wt.%-20wt.%. Adding excess carbonate can ensure the reaction degree of lithium ions in the system, thereby ensuring the Li-containing a X Recovery rate of lithium in the filtrate.

[0042] In the implementation manner of the present application, step (2) also includes the following processing steps:

[0043] c) Residual lithium adsorption treatment: The lithium adsorbent (1-m) Li a X·2Al(OH)3·nH2O is added to the first filtrate, stirred at 20°C-60°C to adsorb lithium ions in the first filtrate, filtered and washed to obtain Li a X·2Al(OH)3·nH2O second precipitation;

[0044] d) Lithium removal: Add the second precipitate into water, stir and react, and filter to obtain (1-m)Li a X·2Al(OH)3·nH2O second lithium adsorbent and filtrate after de-lithiation (i.e., containing Li a X second filtrate);

[0045] e) Lithium precipitation: The filtrate after the above lithium removal is evaporated and concentrated, carbonate is added for stirring reaction, and Li2CO3 precipitate is obtained after filtering and washing.

[0046] Preferably, in the process of adsorbing the residual lithium element in step c), the solid-liquid ratio of the added lithium adsorbent to the first filtrate is 1:(1-30) kg / L. An appropriate amount of lithium adsorbent ensures the adsorption rate of the residual lithium element remaining in the first filtrate. Carrying out the residual lithium adsorption treatment according to the above step c can significantly improve the recovery rate of lithium element in the lithium-containing solution.

[0047] Among them, the parameters in the lithium removal process in step d) can be the same as the parameter range limited by the lithium removal process in step (2), and the parameters in the lithium deposition process in step e) can be the same as the parameter range limited by the lithium deposition process in step (3).

[0048] In some embodiments of the present application, the Li-containing a The second filtrate and the Li-containing a The X filtrates are combined and then evaporated and concentrated in step (3), carbonate is added at a temperature of 50°C-90°C for stirring reaction, and Li2CO3 precipitate is obtained after filtering and washing. In some cases, for example, there is no new Li-containing a When the X filtrate is generated, the Li-containing a After the X filtrates are combined and evaporated and concentrated, production costs can be saved and construction period can be shortened.

[0049] In addition, the lithium adsorbent and the second lithium adsorbent prepared in the above steps can be directly used for the residual lithium adsorption treatment in the process provided in this application, or a part of it can be taken out for drying, and then used in other scenarios for recovering lithium elements, such as the brine adsorption process in the front stage of the salt lake lithium extraction process. Among them, the heating and drying temperature is 70°C-90°C, and the time is 2h-3h. Preferably, the above-mentioned dried lithium adsorbent can be ground or gas-crushed to eliminate the compaction of the powder, so that the lithium adsorbent particles are more delicate and uniform, and its adsorption efficiency in the brine adsorption process is ensured.

[0050] In the embodiment of the present application, the above steps (1), (2) and (3) all include filtering and washing operations, and the washing conditions are: while obtaining the precipitate, the precipitate is sprayed and washed with pure water, and the ratio of the spray water volume per unit time to the precipitate is (0.1-1): 1L / Kg. The appropriate amount of water can effectively remove Na in the precipitate. + , K + It can remove impurity ions such as lithium and will not cause the lithium element in the precipitate to escape, thus ensuring the recovery rate of lithium.

[0051] In the embodiment of the present application, the filtering conditions in the above steps (1), (2) and (3) include: performing the filtering under a vacuum negative pressure of 0.04MPa-0.07MPa, and the mesh number of the filter medium used in the filtering is 300-5000 mesh. The filter medium with the appropriate mesh number and the appropriate vacuum negative pressure conditions can avoid the loss of some tiny particles during the filtering process, thereby ensuring the recovery rate of lithium.

[0052] In some embodiments of the present application, the filtration further includes secondary filtration, and the secondary filtration uses a precision bag filter with an accuracy of 3μm-5μm, which can avoid the problem that the low-mesh filter medium easily allows some fine particles to enter the filtrate and cause the loss of fine particles. The fine particles obtained after the secondary filtration are returned for static aging treatment. Secondary filtration can avoid the loss of fine particles and further improve the recovery rate of lithium.

[0053] In the embodiment of the present application, in step (3), while obtaining Li2CO3, a second filtrate is also obtained, and step (3) further comprises: adding the second filtrate to the lithium-containing solution described in step (1). The above operation can recover the residual lithium element in the second filtrate, further improving the recovery rate of lithium.

[0054] The present application provides a method for recovering lithium from a lithium-containing solution, wherein the lithium element in the lithium-containing solution is separated from the system by forming a precipitate by adjusting the pH value of the lithium-containing solution and adding aluminate, and a large amount of carbonate ions present in the lithium-containing solution are removed at the same time. The precipitate is then treated, filtered, washed and de-lithiated, and while recovering lithium, a recyclable lithium adsorbent with strong adsorption is prepared, and the precipitate obtained in the step is washed to remove a large amount of K entrained in the precipitate. + 、Na + Finally, high-purity Li2CO3 products are prepared by adding carbonate to the filtrate containing lithium elements.

[0055] This method achieves efficient separation of lithium elements and impurity ions, and produces a recyclable lithium adsorbent while recovering lithium, which can achieve further recovery of lithium-containing solutions and has a high recovery rate of lithium in lithium-containing solutions. This method has a simple process, is environmentally friendly, and is convenient for large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0056] Figure 1 This is a process flow chart of lithium recovery in Example 1 of the present application;

[0057] Figure 2 This is a flow chart of the lithium recovery process in Example 2 of the present application. DETAILED DESCRIPTION

[0058] The technical solutions of the embodiments of the present application are described in detail below in multiple embodiments.

[0059] Example 1

[0060] See also Figure 1 The process flow chart shown in the figure recovers lithium from a lithium-containing solution, and specifically includes the following steps.

[0061] (1) Acid neutralization: 10 wt.% HCl solution was slowly added to the lithium-containing solution at a stirring rate of 300 rpm until the pH value dropped to 6.0, and stirring was continued for 0.5 h.

[0062] (2) Aluminum salt precipitation: Prepare 5wt.% NaAlO2 in pure water at a constant temperature of 60°C and a stirring rate of 300rpm, and stir for 30min. At a stirring rate of 300rpm and a constant temperature of 60°C, add the aluminate solution to the aluminum salt solution through a peristaltic pump at a molar ratio of Li:Al of 1.1:2, and the flow rate of the aluminate solution is 500mL / min. Calculate the flow rates of lithium salt and aluminum salt according to the concentrations of the lithium-containing solution and the aluminate solution and the molar ratio of Li:Al. After mixing, continue stirring for 30min to allow the reactants in the solution to react completely.

[0063] (3) Static aging: The solution after the above reaction is further aged at 25°C for 12 hours to obtain a precipitate containing the first precipitate of Li(OH)·2Al(OH)3·nH2O.

[0064] (4) Neutralization transformation: At a stirring rate of 300 rpm, 10 wt.% HCl solution was slowly added to the above precipitate to neutralize it and obtain Li a X·2Al(OH)3·nH2O precipitation. Monitor the pH value during the acid addition process until the pH value is adjusted to 6.0 and continue stirring for 30 minutes.

[0065] (5) Filtration and washing 1: Filter through a vacuum filter with a 500-mesh filter cloth at a vacuum negative pressure of 0.04 MPa to filter out the precipitate. While filtering, spray the filtrate with pure water, and the ratio of the spray water volume to the lithium adsorbent per unit time is 0.5 L / Kg. The filtrate after filtration and washing is filtered again through a precision bag filter with a filter accuracy of 3 μm.

[0066] The collected fine particles are returned to the aging process to obtain the first filtrate.

[0067] (6) Lithium removal: Filter and wash the Li a X·2Al(OH)3·nH2O was mixed with water in a mass ratio of 1:20, kept at 40°C, and stirred at 300 rpm for 3 h. Filtered and washed to obtain the lithium adsorbent (1-m)Li a X·2Al(OH)3·nH2O (D50 particle size is 36.86μm) and Li-containing a X filtrate. The filter medium mesh is 500 mesh, and the vacuum pressure of the filter is 0.04MPa. The filtered filtrate is filtered again through a precision bag filter with a filter accuracy of 3μm. The collected fine particles are returned for aging treatment.

[0068] (7) Lithium precipitation: First, evaporate and concentrate the Li a The X filtrate was evaporated and concentrated to make the lithium concentration in the filtrate 22g / L. The evaporated and concentrated solution was heated to 90°C and kept at a constant temperature. 10wt.% Na2CO3 was added at a stirring rate of 300rpm, and the addition amount was 1.2 times the theoretical calculated amount. After the addition was completed, stirring was continued for 0.5h, and then allowed to stand for 2h.

[0069] (8) Filtration and washing 2: Filter out the Li2CO3 precipitate through a vacuum filter, the mesh size of the filter medium is 300 mesh, and the vacuum negative pressure of the filter is 0.04 MPa. While filtering, spray wash the filtrate with pure water, and the ratio of the spray water volume to Li2CO3 per unit time is 0.5 L / Kg. The obtained second filtrate is added to the lithium-containing solution of step (1).

[0070] (9) Drying: The filtrate was dried in a forced air drying oven at 130° C. for 120 min to obtain a Li2CO3 product.

[0071] The method further includes a treatment for adsorption of residual lithium: adding the precipitate (i.e., lithium adsorbent) after delithiation (6) to the first filtrate containing residual lithium obtained in step (5) at a stirring rate of 300 rpm, wherein the solid-liquid ratio of the lithium adsorbent to the first filtrate is 1:20 (i.e., 1 kg of adsorbent is added to every 20 L of filtrate), and stirring is performed at a constant temperature of 40°C for 90 minutes.

[0072] Filtration and washing 3: The tail liquid after the residual lithium adsorption is passed through a vacuum filter with a filter medium mesh of 500 mesh and a filter vacuum negative pressure of 0.04MPa. Filter out the LiCl·2Al(OH)3·nH2O after the residual lithium adsorption, and spray the filtrate with pure water while filtering. The ratio of spray water volume to adsorbent per unit time is 0.5L / Kg. The filtrate is de-lithiumed, and the filtrate is filtered again through a precision bag filter with a filter accuracy of 3μm. The filtered filtrate is returned for aging treatment and the filtrate is discharged. Li a X·2Al(OH)3·nH2O second precipitation.

[0073] The second precipitate is mixed with water and stirred to perform the above-mentioned lithium removal reaction to obtain the second lithium adsorbent (1-m)Li a X·2Al(OH)3·nH2O (D50 particle size is 36.86μm) and Li-containing a X second filtrate (the process parameters in this process are the same as those used for lithium removal in step (6)).

[0074] Will contain Li aThe second filtrate is treated with lithium precipitation, and Li2CO3 is obtained by filtering, washing and drying (the process parameters in this process are the same as those used in the above steps (7) lithium precipitation, (8) filtering and washing 2, and (9) drying).

[0075] Example 2

[0076] See also Figure 2 The process flow chart shown in the figure recovers lithium from a lithium-containing solution, and specifically includes the following steps.

[0077] (1) Aluminum salt precipitation: Prepare 5wt.% NaAlO2 in pure water at a constant temperature of 60°C and a stirring rate of 300rpm, and stir for 30min. At a stirring rate of 300rpm and a constant temperature of 60°C, add the aluminate solution into the aluminum salt solution through a peristaltic pump at a molar ratio of Li:Al of 1.1:2, and the flow rate of the aluminate solution is 500mL / min. Calculate the flow rates of lithium salt and aluminum salt according to the concentrations of the lithium-containing solution and the aluminate solution and the molar ratio of Li:Al. Slowly add 10wt.% HCl solution into the lithium-containing solution until the pH value drops to 6.0. After mixing, continue stirring for 30min to allow the reactants in the solution to react completely to obtain Li a X·2Al(OH)3·nH2O precipitation.

[0078] The subsequent static aging, filtration and washing 1, residual lithium adsorption, lithium removal, lithium precipitation, filtration and washing 2, filtration and washing 3 and drying operations are the same as those in Example 1. A lithium adsorbent (1-m)Li with a D50 particle size of 40.11 μm is obtained. a X·2Al(OH)3·nH2O.

[0079] Example 3

[0080] The difference between Example 3 and Example 1 is that during the aluminum salt precipitation process in step (2), the molar ratio of Li:Al is 1.3:2, and the other conditions and operations are consistent with those in Example 1. The lithium adsorbent (1-m) Li with a D50 particle size of 41.28 μm is obtained. a X·2Al(OH)3·nH2O.

[0081] Example 4

[0082] The difference between Example 4 and Example 1 is that during the aluminum salt precipitation process in step (2), the molar ratio of Li:Al is 1.2:2, and the other conditions and operations are consistent with those in Example 1. A lithium adsorbent (1-m) Li with a D50 particle size of 38.19 μm is obtained. a X·2Al(OH)3·nH2O.

[0083] Example 5

[0084] The difference between Example 5 and Example 1 is that during the lithium removal process in step (6), the temperature is controlled at 20°C, and the other conditions and operations are consistent with those in Example 1. A lithium adsorbent (1-m) Li with a D50 particle size of 43.87 μm is obtained. a X·2Al(OH)3·nH2O.

[0085] Example 6

[0086] The difference between Example 6 and Example 1 is that during the lithium removal process in step (6), the temperature is controlled to be 60°C, and the other conditions and operations are consistent with those in Example 1. A lithium adsorbent (1-m) Li with a D50 particle size of 40.41 μm is obtained. a X·2Al(OH)3·nH2O.

[0087] Example 7

[0088] The difference between Example 7 and Example 1 is that during the lithium precipitation process in step (7), the amount of Na2CO3 added is 1.05 times the theoretical amount, and the other conditions and operations are consistent with those in Example 1. A lithium adsorbent (1-m) Li with a D50 particle size of 37.13 μm is obtained. a X·2Al(OH)3·nH2O.

[0089] Example 8

[0090] The difference between Example 8 and Example 1 is that during the lithium precipitation process in step (7), the amount of Na2CO3 added is 1.3 times the theoretical amount, and the other conditions and operations are consistent with those in Example 1. A lithium adsorbent (1-m) Li with a D50 particle size of 39.51 μm is obtained. a X·2Al(OH)3·nH2O.

[0091] Example 9

[0092] Compared with Example 1, the pressure of all vacuum filtrations was adjusted to 0.06 MPa, and other conditions remained unchanged. A lithium adsorbent (1-m)Li with a D50 particle size of 44.64 μm was obtained. a X·2Al(OH)3·nH2O.

[0093] Example 10

[0094] Example 10 Compared with Example 1, the secondary filtration step of filtering and washing-1, filtering, and filtering and washing-3 by using a precision bag filter was removed, and other conditions remained unchanged. A lithium adsorbent (1-m)Li with a D50 particle size of 35.49 μm was obtained. a X·2Al(OH)3·nH2O.

[0095] Embodiment 11

[0096] The difference between Example 11 and Example 1 is that in step (4) and after the transformation, no lithium adsorbent is used to adsorb the residual lithium in the first filtrate, and the residual lithium is directly discharged after precision filtration. The lithium adsorbent (1-m) Li with a D50 particle size of 38.11 μm is obtained. a X·2Al(OH)3·nH2O.

[0097] The technical solution provided by the present application is evaluated from the perspectives of lithium recovery rate, Li2CO3 purity, adsorption capacity of lithium adsorbent and lithium concentration in the effluent. The lithium recovery rate is calculated based on the lithium concentration (Li + The concentration of Li2CO3 was calculated by measuring the content of carbonate by potentiometric titration, and the concentration of lithium in the effluent was measured by inductively coupled plasma (ICP) spectrometer. The test results of each embodiment are recorded in Table 1.

[0098] The method for testing the adsorption capacity of lithium adsorbent is as follows: take lithium-containing brine with a high magnesium-lithium ratio for testing, Li + The concentration is 0.0233wt.%Mg 2+ The concentration is 7.8540wt.%, and the mass ratio of Mg:Li in the brine is 337:1. Weigh 10g of lithium adsorbent and adsorb it at a solid-liquid ratio of 1:50 at room temperature, with a stirring rate of 300rpm and an adsorption time of 90min. The concentration difference of lithium in the brine before and after adsorption is the adsorption capacity of the lithium adsorbent.

[0099] Table 1 Test results of embodiments and comparative examples

[0100]

[0101]

[0102] The results of the various tests of Examples 1-11 in Table 1 are compared below:

[0103] (1) The test results of Examples 1 and 2 are compared: the adsorption capacity of the lithium adsorbent prepared in Example 2 is lower than that in Example 1, but since the residual lithium content of the first filtrate in Example 2 is lower than that in Example 1, the final recovery rates of lithium element in the above two examples are not much different.

[0104] (2) Comparing the test results of Examples 1, 3, and 4: In the aluminum salt precipitation step, an appropriate excess of lithium in the lithium-containing solution is conducive to the complete reaction of the metaaluminate, and no aluminum element remains in the system after the reaction, thereby improving the purity of lithium carbonate. However, too much excess lithium will lead to a decrease in the lithium recovery rate.

[0105] (3) Comparing the test results of Examples 1, 5, and 6: At the same time, the delithiation temperature is low, the amount of lithium removed is low, resulting in a lower lithium recovery rate and a decrease in the adsorption capacity of the adsorbent. The delithiation temperature is high, the amount of lithium desorbed is large, and the lithium recovery rate is high, but too high a temperature may lead to excessive delithiation, resulting in damage to the adsorbent structure, which in turn leads to a decrease in adsorption capacity.

[0106] (4) Comparing the test results of Examples 1, 7, and 8: A proper excess of sodium carbonate can ensure the degree of reaction of lithium ions in the system, thereby improving the recovery rate of lithium. However, if the sodium carbonate is excessive, the sodium ion concentration increases, resulting in a decrease in the purity of lithium carbonate.

[0107] (5) Comparing the test results of Examples 1 and 9, increasing the negative pressure of vacuum filtration can improve the purity of the obtained Li2CO3.

[0108] (6) Comparison of the test results of Examples 1 and 10: The secondary filtration can avoid the loss of fine particles, further improve the lithium recovery rate, and prevent fine particles from entering the lithium precipitation step, resulting in a decrease in the purity of lithium carbonate.

[0109] (7) The test results of Examples 1 and 11 were compared: Compared with Example 1, Example 10 did not perform adsorption treatment on the residual lithium element remaining in the first filtrate, and the recovery rate was significantly reduced.

[0110] The above is an exemplary embodiment of the present application. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications are also considered to be within the scope of protection of the present application.

Claims

1. A method for recovering lithium from a lithium-containing solution, characterized in that: The following steps are involved: (1) precipitating lithium from a lithium-containing solution in the following manner a) or b): the lithium-containing solution is a lithium precipitation mother solution; a) adjusting the pH of the lithium-containing solution to 5-6 and then mixing it with the aluminate solution, allowing it to stand for aging to obtain a precipitate containing the first precipitate of Li(OH)·2Al(OH)3·nH2O, wherein n=1-3; The pH value of the precipitate is adjusted to 6-7, and then filtered and washed to obtain Li a X·2Al(OH)3·nH2O precipitate and first filtrate; b) Mixing the lithium-containing solution with the aluminate solution and adjusting the pH of the system to 5-7, allowing the reaction to stand for aging, filtering and precipitating to obtain Li a X·2Al(OH)3·nH2O precipitate and first filtrate; Wherein, X represents the anion of the acid solution used to adjust the pH, and a = 1 or 2; (2) Lithium removal: a X·2Al(OH)3·nH2O precipitate was added to water and stirred for reaction, and the lithium adsorbent (1-m)Li was obtained by filtration. a X·2Al(OH)3·nH2O and Li a X filtrate, wherein m=0.1-0.9; the conditions for removing lithium include: the Li a The X·2Al(OH)3·nH2O precipitate is mixed with water in a mass ratio of 1:(1-50) and stirred at 20℃-60℃ for 1h-24h; (3) Lithium precipitation: a The X filtrate is evaporated and concentrated, carbonate is added for stirring reaction, and Li2CO3 precipitate is obtained after filtering and washing; Wherein, the Li-containing a The molar ratio of lithium element in the X filtrate to carbonate ion in the carbonate is (1.05-1.3):2; (4) adding the lithium adsorbent to the first filtrate, stirring at 20°C-60°C to adsorb the lithium ions in the first filtrate, filtering and washing to obtain Li a X·2Al(OH)3·nH2O second precipitation; The second precipitate is subjected to the delithiation and the filtrate after the delithiation is subjected to the lithium precipitation.

2. The method according to claim 1, characterized in that The acid solution is one of sulfuric acid, hydrochloric acid, nitric acid or acetic acid.

3. The method according to claim 1, characterized in that The D50 particle size of the lithium adsorbent is 20 μm-100 μm.

4. The method according to claim 1, characterized in that: The Li-containing a The X filtrate is evaporated and concentrated to a lithium concentration of 15 g / L-25 g / L.

5. The method according to claim 1, characterized in that In step (3), the carbonate is added to the Li-containing a X filtrate.

6. The method according to claim 1, characterized in that Step (1) also includes: when adjusting the pH, collecting carbon dioxide generated by the lithium-containing solution and passing it into an alkaline solution to obtain carbonate; wherein the alkaline solution is NaOH or KOH, and the carbonate is Na2CO3 or K2CO3.

7. The method according to claim 1, characterized in that In step (1), the lithium-containing solution and the aluminate are mixed in a molar ratio of Li:Al of (1.05-1.3):

2.

8. The method according to claim 1, characterized in that: In step (3), while obtaining the Li2CO3 precipitate, a second filtrate is also obtained, and the method further comprises: adding the second filtrate to the lithium-containing solution.

9. The method according to claim 1, characterized in that: The filtering conditions include: performing the filtering under a vacuum negative pressure of 0.04 MPa-0.07 MPa, and the mesh number of the filtering medium used in the filtering is 300-5000 mesh.