Noise-reducing polycarbonate composition and preparation method thereof
By using maleic anhydride-grafted ABS and methacrylic acid-butadiene-styrene terpolymer as compatibilizers in PC/ABS alloy, combined with low damping materials TDI and MDI copolymerized TPU and silicone masterbatch, It solves the noise problem of automobile interior parts, achieves excellent mechanical properties and low odor characteristics of the material, and is suitable for automobile interior and exterior parts.
Patent Information
- Application Number
- CN202211594446.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-13
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-12-13
AI Technical Summary
The noise problem caused by friction of existing PC/ABS alloys in automotive interior parts has not been effectively solved, and commonly used noise reduction materials have a negative impact on material performance and appearance, and there is a lack of solutions with low odor and excellent mechanical properties.
Maleic anhydride grafted ABS and methacrylic acid-butadiene-styrene terpolymer are used as compatibilizers, combined with low damping materials TDI and MDI copolymerized TPU and noise reduction additive silicone masterbatch, through feeding The extruder and parallel twin-screw extruder are used for melt extrusion and granulation to improve the compatibility and noise reduction performance of the material.
It reduces the damping coefficient and surface friction coefficient of the material, while improving the mechanical properties and processability. It is suitable for automotive interior and exterior parts, and the amount of TPU resin is reduced to maintain the overall temperature resistance of the material.
Smart Images

Figure SMS_1 
Figure SMS_10 
Figure SMS_11
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer materials, and particularly relates to a noise-reducing polycarbonate composition and a preparation method thereof. Background Art
[0002] PC / ABS alloy is a polymer material widely used in automobiles. With the vibration of the car, the interior parts made of PC / ABS alloy or the parts of other materials rub and collide with each other, sometimes making a squeaking sound. With the improvement of public environmental awareness and self-protection awareness, passengers have stricter requirements for driving experience and comfortable and healthy in-car environment. Improving the level of vehicle noise control and reducing the emission of odor in the car have become new competition focuses, technical development directions and important market selling points.
[0003] In order to reduce noise, the common solution is to apply grease to the joints of components during the automobile assembly process, or to stick velvet or sponge in household appliances. Although there is a certain improvement effect, it cannot permanently prevent abnormal noise, and the effect does not last when placed at high temperature for a long time. At present, there is no low-odor PC / ABS alloy for noise reduction in the automotive industry. The noise reduction materials in related industries are mostly filled and multi-layered, which is not conducive to the processability and aesthetic requirements of product parts.
[0004] After consulting many literatures and patents, the common modification ideas for the material side of this problem are summarized as follows:
[0005] 1. By adding lubricating additives to reduce the friction coefficient of the surface of the workpiece, the abnormal noise can be eliminated or weakened. However, most lubricants are incompatible with the PC / ABS system and will still precipitate after long-term use, thus eliminating the effect of preventing abnormal noise.
[0006] 2. By improving the damping performance of the material, the energy generated by friction vibration is dissipated in the form of internal energy to achieve the purpose of preventing abnormal noise. For example, TPU is introduced in CN107177156A and CN107325514A to improve the damping effect of the material to achieve the purpose of noise reduction. The results show that the effect is very significant, but the introduction of excessive TPU will significantly deteriorate the physical properties of the material, and the material is easy to delaminate during the injection molding process. In addition, CN 111303580A introduces lamellar graphite to enhance the storage modulus of the material, thereby improving the damping property of the material, but 20 parts of graphite will not only have a negative impact on the impact toughness of the material, but the black graphite will affect the color matching of light-colored interior parts, thereby limiting its wide application.
[0007] 3. For example, Guo Shaoyun et al., in patent CN102501504A, put two different polymer materials into an extruder for multi-layer extrusion to achieve the effect of noise reduction; Xu Bo et al., in patent CN102967042B, put double-sided tape between polyurethane sponge and melamine sponge, and then heat-pressed composite to achieve the effect of sound absorption. However, the use of such multi-layer extrusion or hot-pressed composite methods will be restricted by the appearance of the product, especially in the case of the current diversified interior structure design of the car, these methods cannot be well applied to parts with complex structures.
[0008] TPU 1180 commercialized by BASF of Germany is a very unique TDI and MDI copolymer polyurethane resin with extremely high shock absorption and damping properties. Introducing this structure into the PC / ABS system will also improve the damping performance of the material in theory. However, commonly used triblock copolymers such as SBS (styrene-butadiene-styrene), SEBS (hydrogenated SBS) and SIS (styrene-isoprene-styrene) have poor compatibility with the PC / ABS system. Therefore, the PC / ABS / TPU system will be delaminated. The compatibilizer used in the present invention is one or more of maleic anhydride grafted ABS and methacrylic acid-butadiene-styrene terpolymer, which can effectively improve the compatibility problem between several base resins. Summary of the invention
[0009] Based on this, one of the purposes of the present invention is to provide a noise reduction polycarbonate composition, which has excellent mechanical properties, fluidity, and low odor while having noise reduction performance, and can be used in industries such as automotive interior and exterior decoration.
[0010] The specific technical solutions for achieving the above-mentioned invention objectives include the following:
[0011] A noise reduction polycarbonate composition is prepared from the following raw materials in parts by weight:
[0012]
[0013] Wherein, the total weight of the polycarbonate resin, the polyurethane resin and the acrylonitrile-butadiene-styrene copolymer is 100 parts;
[0014] In some embodiments, the noise reduction polycarbonate composition is prepared from the following raw materials in parts by weight:
[0015]
[0016]
[0017] In some embodiments, the polycarbonate composition is preferably prepared from the following raw materials in parts by weight:
[0018]
[0019] In some embodiments, the compatibilizer is at least one of maleic anhydride grafted ABS and methacrylic acid-butadiene-styrene terpolymer.
[0020] The compatibilizer in the present invention is a polymer compatibilizer having polar functional groups in the molecule in order to enhance the interface bonding between PC and ABS and improve the mechanical properties of the material.
[0021] The styrene-acrylonitrile-glycidyl methacrylate copolymer is of a reactive type, wherein the mass fraction of glycidyl methacrylate is 2wt% to 4wt%.
[0022] In some embodiments, the polycarbonate resin is bisphenol A polycarbonate, and its melt index is 10 g / 10 min to 12 g / 10 min at 300° C. / 1.2 kg.
[0023] In some embodiments, the polyurethane resin is a copolymer of TDI and MDI.
[0024] In some embodiments, the noise reduction agent is GM-100 silicone masterbatch.
[0025] In some embodiments, the hindered phenol antioxidant is β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate octadecyl alcohol, and / or the phosphite antioxidant is bis(2,6-di-tert-butyl-4-methylphenyl) pentaerythritol diphosphate.
[0026] Another object of the present invention is to provide a method for preparing the above-mentioned noise reduction polycarbonate composition, which comprises the following steps:
[0027] (1) mixing the dried polycarbonate resin, polyurethane resin, acrylonitrile-butadiene-styrene copolymer, a compatibilizer, a noise reduction agent and styrene-acrylonitrile-glycidyl methacrylate copolymer to obtain a mixture A;
[0028] (2) mixing a hindered phenol antioxidant, a phosphite antioxidant and pentaerythritol stearate to obtain a mixture B;
[0029] (3) Mixing mixture A and mixture B again to obtain mixture C;
[0030] (4) The mixture C is fed into a parallel twin-screw extruder via a feeder, and melt-extruded and granulated to obtain a noise-reducing polycarbonate composition.
[0031] In some embodiments, the process parameters of the melt extrusion granulation include: the temperature of zone 1 is 210℃~240℃, the temperature of zone 2 is 230℃~260℃, the temperature of zone 3 is 235℃~260℃, the temperature of zone 4 is 220℃~260℃, the temperature of zone 5 is 220℃~260℃, the temperature of zone 6 is 220℃~260℃, the temperature of zone 7 is 220℃~260℃, the temperature of zone 8 is 220℃~260℃, the die head temperature is 240℃~275℃, and the screw speed is 200rpm~600rpm.
[0032] In some of the embodiments, the process parameters of the melt extrusion granulation include: the temperature of zone 1 is 225℃~235℃, the temperature of zone 2 is 235℃~245℃, the temperature of zone 3 is 245℃~255℃, the temperature of zone 4 is 245℃~255℃, the temperature of zone 5 is 245℃~255℃, the temperature of zone 6 is 245℃~255℃, the temperature of zone 7 is 240℃~250℃, the temperature of zone 8 is 240℃~250℃, the die head temperature is 255℃~265℃, and the screw speed is 350rpm~500rpm.
[0033] In some embodiments, the drying conditions in step (1) include: a temperature of 80° C. to 110° C. and a time of 4 hours to 8 hours.
[0034] In some embodiments, the drying conditions in step (1) include: a temperature of 100° C. to 110° C. and a time of 4 to 6 hours.
[0035] In some embodiments, the stirring speed of the mixing in step (1) is 400 rpm to 600 rpm.
[0036] In some embodiments, the stirring speed of the mixing in step (2) is 400 rpm to 600 rpm.
[0037] In some embodiments, the mixing in step (3) is performed at a stirring speed of 400 to 600 rpm, and the stirring time is 8 to 12 min.
[0038] In some embodiments, the screw shape of the parallel twin-screw extruder is a single-line screw.
[0039] In some of the embodiments, the ratio L / D of the screw length L to the diameter D of the parallel twin-screw extruder is 35 to 50; and the screw is provided with more than one meshing block area and more than one reverse thread area.
[0040] In some embodiments, the ratio L / D of the screw length L to the screw diameter D is 35-45; and the screw is provided with two meshing block areas and one reverse thread area.
[0041] Different from the traditional PC / ABS alloy, the present invention uses TDI and MDI type copolymerized polyurethane (TPU) and noise reduction agent silicone masterbatch to compound noise reduction, wherein TPU as a green low damping material can effectively improve the damping coefficient of the material, but only a large amount of use can effectively reduce the damping coefficient of the material, and at the same time, because TPU has poor compatibility with PC and ABS resin matrix components, the addition of too much TPU resin will cause the mechanical properties of the material to deteriorate, reduce temperature resistance, and injection molding delamination and other problems. Therefore, a compatibilizer is added in the present application to improve the problem. Compared with the traditional methyl methacrylate-styrene-butadiene copolymer, the compatibilizer maleic anhydride grafted ABS or methacrylic acid-butadiene-styrene terpolymer has been surface-modified by maleic anhydride or silane coupling agent, which can effectively coordinate the compatibility between different matrixes in the formula, thereby achieving the purpose of improving the mechanical properties of the material, and can make the polycarbonate composition have higher toughness, so that the material can be used in more severe environments for a longer period of time without deformation. Although the addition of compatibilizer can effectively improve the mechanical properties of the material, the addition of excessive TPU resin will still reduce the overall temperature resistance of the material. Therefore, the compounding of noise reduction additive and TPU resin in the present invention can not only achieve the effect of further noise reduction, but also effectively reduce the amount of TPU resin, thereby reducing the decline in the overall temperature resistance of the material. The introduction of noise reduction additive silicone masterbatch, which belongs to the silane series lubricant, reduces the surface friction coefficient of the material and reduces the noise generated by friction when the products are in contact with each other.
[0042] The antioxidant β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate octadecyl ester in the present invention has good thermal stability in the process of blending the polycarbonate composition, and the hindered piperidine group of the antioxidant can provide antioxidant effect and improve the dyeability of the copolymer; the melting point of bis(2,6-di-tert-butyl-4-methylphenyl) pentaerythritol diphosphate is 239°C, the thermal decomposition temperature exceeds 350°C, and it has good heat resistance and hydrolysis resistance, and can provide excellent color stability and melting stability for the modified polycarbonate material in the process of high-speed blending, and can prevent the thermal degradation of polycarbonate, flame retardant and other small molecule additives in the high temperature process, and can inhibit the thermal oxidative discoloration caused by long time, and it also provides nitrogen oxides (NO x ) Color stability in gas environment to prevent gas fumigation discoloration.
[0043] The present invention adopts pentaerythritol stearate to improve the demoulding property of the material and increase the thermal stability. When it is used alone as a lubricant, it can effectively reduce the shear force of the screw on the material and reduce the performance damage of the material caused by physical shearing.
[0044] Compared with the prior art, the present invention has the following beneficial effects:
[0045] The present invention uses a low damping material TDI and MDI copolymer TPU and a noise reduction auxiliary agent silicone masterbatch to effectively reduce the damping coefficient and surface friction coefficient of the material; by adding grafted maleic anhydride grafted ABS and methacrylic acid-butadiene-styrene terpolymer to improve the mechanical properties of the polycarbonate composition and improve the compatibility between different resin matrices, so that the product will not be delaminated during the material injection molding process due to the presence of three different resins. In addition, compared with the polycarbonate material, the addition of TPU resin and acrylonitrile-butadiene-styrene copolymer has a lower melting temperature, which makes the modified material have a lower processing temperature, so that the improved polycarbonate composition has better processability.
[0046] The raw material components of the present invention cooperate with each other so that the obtained noise reduction polycarbonate composition has excellent low damping performance, surface friction coefficient, mechanical properties and processing performance, and is suitable for automobile products.
[0047] The preparation method of the noise reduction polycarbonate composition provided by the invention has simple process, is easy to control, has low requirements on equipment, and the equipment used is all general polymer processing equipment, has low investment, and is conducive to industrial production. DETAILED DESCRIPTION
[0048] In order to facilitate the understanding of the present invention, the present invention will be described more fully below. The present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0049] Unless otherwise defined, all technical and scientific terms used in the present invention have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used in the present invention includes any and all combinations of one or more of the related listed items.
[0050] The raw materials used in the examples and comparative examples of the present invention are as follows:
[0051] Polycarbonate resin, with a weight average molecular weight of 17000-19000 and a melt index of 10 g / 10 min, selected from Teijin Co., Ltd. of Japan;
[0052] The acrylonitrile-butadiene-styrene copolymer comprises 5-30% acrylonitrile, 10-30% acrylonitrile and 40-70% styrene in mass percentage; the ABS resin has a number average molecular weight of 80,000-150,000 g / mol and is selected from Shanghai Gaoqiao.
[0053] Polyurethane resin, TDI and MDI copolymer TPU, selected from BASF of Germany;
[0054] The noise reduction agent silicone masterbatch is selected from GM-100, which is selected from Sichuan Chenguang Chemical;
[0055] Compatibilizer EM-500, selected from LG Chem of South Korea;
[0056] Styrene-acrylonitrile-glycidyl methacrylate copolymer, the mass fraction of glycidyl methacrylate (GMA) is 3wt%, selected from Sigma-Aldrich (Shanghai) Trading Co., Ltd.;
[0057] β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, selected from BASF GmbH, Germany;
[0058] Bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphate, selected from Shanghai Dianyao Fine Chemical Co., Ltd.;
[0059] Pentaerythritol stearate, selected from Zhaoqing Sendeli Chemical Industry Co., Ltd.;
[0060] The present invention is described in detail below with reference to specific embodiments.
[0061] Example 1
[0062] A noise reduction polycarbonate composition of this embodiment is prepared from the following raw materials in parts by weight:
[0063]
[0064] The method for preparing the noise reduction polycarbonate composition of this embodiment comprises the following steps:
[0065] (1) The polycarbonate resin, polyurethane resin, and acrylonitrile-butadiene-styrene copolymer are dried at 120° C., 70° C., and 80° C., respectively. After 4 hours, they are cooled and added into a mixer (with a rotation speed of 500 rpm) together with a compatibilizer, a noise reduction agent, and a styrene-acrylonitrile-glycidyl methacrylate copolymer for mixing.
[0066] (2) Add β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate octadecyl ester, bis(2,6-di-tert-butyl-4-methylphenyl) pentaerythritol diphosphate, and pentaerythritol stearate into another mixer (rotating speed is 500 rpm) and mix.
[0067] (3) Pour the mixture obtained in step (1) and step (2) into the same high-speed mixer (rotation speed is 500 rpm) and mix for 10 min.
[0068] (4) adding the mixed material in step (3) into a parallel twin-screw extruder through a feeder, and performing melt extrusion granulation in the parallel twin-screw extruder (eight zones in total), wherein the process parameters include: a temperature of zone 1 of 230° C., a temperature of zone 2 of 240° C., a temperature of zone 3 of 250° C., a temperature of zone 4 of 250° C., a temperature of zone 5 of 250° C., a temperature of zone 6 of 250° C., a temperature of zone 7 of 245° C., a temperature of zone 8 of 245° C., a die head temperature of 260° C., and a screw speed of 500 rpm; the screw shape of the parallel twin-screw extruder is a single-threaded screw, the ratio of screw length L to diameter D (L / D) is 35, and the screw is provided with two meshing block zones and one reverse thread zone.
[0069] Example 2
[0070] A noise reduction polycarbonate composition of this embodiment is prepared from the following raw materials in parts by weight:
[0071]
[0072] The method for preparing the noise reduction polycarbonate composition of this embodiment comprises the following steps:
[0073] (1) The polycarbonate resin, polyurethane resin, and acrylonitrile-butadiene-styrene copolymer are dried at 120° C., 70° C., and 80° C., respectively. After 4 hours, they are cooled and added into a mixer (with a rotation speed of 500 rpm) together with a compatibilizer, a noise reduction agent, and a styrene-acrylonitrile-glycidyl methacrylate copolymer for mixing.
[0074] (2) Add β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate octadecyl ester, bis(2,6-di-tert-butyl-4-methylphenyl) pentaerythritol diphosphate, and pentaerythritol stearate into another mixer (rotating speed is 500 rpm) and mix.
[0075] (3) Pour the mixture obtained in step (1) and step (2) into the same high-speed mixer (rotation speed is 500 rpm) and mix for 10 min.
[0076] (4) adding the mixed material in step (3) into a parallel twin-screw extruder through a feeder, and performing melt extrusion granulation in the parallel twin-screw extruder (eight zones in total), wherein the process parameters include: a temperature of zone 1 of 230° C., a temperature of zone 2 of 240° C., a temperature of zone 3 of 250° C., a temperature of zone 4 of 250° C., a temperature of zone 5 of 250° C., a temperature of zone 6 of 250° C., a temperature of zone 7 of 245° C., a temperature of zone 8 of 245° C., a die head temperature of 260° C., and a screw speed of 500 rpm; the screw shape of the parallel twin-screw extruder is a single-threaded screw, the ratio of screw length L to diameter D (L / D) is 35, and the screw is provided with two meshing block zones and one reverse thread zone.
[0077] Example 3
[0078] A noise reduction polycarbonate composition of this embodiment is prepared from the following raw materials in parts by weight:
[0079]
[0080]
[0081] The method for preparing the noise reduction polycarbonate composition of this embodiment comprises the following steps:
[0082] (1) The polycarbonate resin, polyurethane resin, and acrylonitrile-butadiene-styrene copolymer are dried at 120° C., 70° C., and 80° C., respectively. After 4 hours, they are cooled and added into a mixer (with a rotation speed of 500 rpm) together with a compatibilizer, a noise reduction agent, and a styrene-acrylonitrile-glycidyl methacrylate copolymer for mixing.
[0083] (2) Add β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate octadecyl ester, bis(2,6-di-tert-butyl-4-methylphenyl) pentaerythritol diphosphate, and pentaerythritol stearate into another mixer (rotating speed is 500 rpm) and mix.
[0084] (3) Pour the mixture obtained in step (1) and step (2) into the same high-speed mixer (rotation speed is 500 rpm) and mix for 10 min.
[0085] (4) adding the mixed material in step (3) into a parallel twin-screw extruder through a feeder, and performing melt extrusion granulation in the parallel twin-screw extruder (eight zones in total), wherein the process parameters include: a temperature of zone 1 of 230° C., a temperature of zone 2 of 240° C., a temperature of zone 3 of 250° C., a temperature of zone 4 of 250° C., a temperature of zone 5 of 250° C., a temperature of zone 6 of 250° C., a temperature of zone 7 of 245° C., a temperature of zone 8 of 245° C., a die head temperature of 260° C., and a screw speed of 500 rpm; the screw shape of the parallel twin-screw extruder is a single-threaded screw, the ratio of screw length L to diameter D (L / D) is 35, and the screw is provided with two meshing block zones and one reverse thread zone.
[0086] Example 4
[0087] A noise reduction polycarbonate composition of this embodiment is prepared from the following raw materials in parts by weight:
[0088]
[0089]
[0090] The method for preparing the noise reduction polycarbonate composition of this embodiment comprises the following steps:
[0091] (1) The polycarbonate resin, polyurethane resin, and acrylonitrile-butadiene-styrene copolymer are dried at 120° C., 70° C., and 80° C., respectively, cooled after 4 hours, and then added into a mixer (with a rotation speed of 500 rpm) together with a compatibilizer, a noise reduction agent, and a styrene-acrylonitrile-glycidyl methacrylate copolymer for mixing.
[0092] (2) Add β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate octadecyl ester, bis(2,6-di-tert-butyl-4-methylphenyl) pentaerythritol diphosphate, and pentaerythritol stearate into another mixer (rotating speed is 500 rpm) and mix.
[0093] (3) Pour the mixture obtained in step (1) and step (2) into the same high-speed mixer (rotation speed is 500 rpm) and mix for 10 min.
[0094] (4) adding the mixed material in step (3) into a parallel twin-screw extruder through a feeder, and performing melt extrusion granulation in the parallel twin-screw extruder (eight zones in total), wherein the process parameters include: a temperature of zone 1 of 230° C., a temperature of zone 2 of 240° C., a temperature of zone 3 of 250° C., a temperature of zone 4 of 250° C., a temperature of zone 5 of 250° C., a temperature of zone 6 of 250° C., a temperature of zone 7 of 245° C., a temperature of zone 8 of 245° C., a die head temperature of 260° C., and a screw speed of 500 rpm; the screw shape of the parallel twin-screw extruder is a single-threaded screw, the ratio of screw length L to diameter D (L / D) is 35, and the screw is provided with two meshing block zones and one reverse thread zone.
[0095] Example 5
[0096] A noise reduction polycarbonate composition of this embodiment is prepared from the following raw materials in parts by weight:
[0097]
[0098]
[0099] The method for preparing the noise reduction polycarbonate composition of this embodiment comprises the following steps:
[0100] (1) The polycarbonate resin, polyurethane resin, and acrylonitrile-butadiene-styrene copolymer are dried at 120° C., 70° C., and 80° C., respectively. After 4 hours, they are cooled and added into a mixer (with a rotation speed of 500 rpm) together with a compatibilizer, a noise reduction agent, and a styrene-acrylonitrile-glycidyl methacrylate copolymer for mixing.
[0101] (2) Add β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate octadecyl ester, bis(2,6-di-tert-butyl-4-methylphenyl) pentaerythritol diphosphate, and pentaerythritol stearate into another mixer (rotating speed is 500 rpm) and mix.
[0102] (3) Pour the mixture obtained in step (1) and step (2) into the same high-speed mixer (rotation speed is 500 rpm) and mix for 10 min.
[0103] (4) adding the mixed material in step (3) into a parallel twin-screw extruder through a feeder, and performing melt extrusion granulation in the parallel twin-screw extruder (eight zones in total), wherein the process parameters include: a temperature of zone 1 of 230° C., a temperature of zone 2 of 240° C., a temperature of zone 3 of 250° C., a temperature of zone 4 of 250° C., a temperature of zone 5 of 250° C., a temperature of zone 6 of 250° C., a temperature of zone 7 of 245° C., a temperature of zone 8 of 245° C., a die head temperature of 260° C., and a screw speed of 500 rpm; the screw shape of the parallel twin-screw extruder is a single-threaded screw, the ratio of screw length L to diameter D (L / D) is 35, and the screw is provided with two meshing block zones and one reverse thread zone.
[0104] Example 6
[0105] A noise reduction polycarbonate composition of this embodiment is prepared from the following raw materials in parts by weight:
[0106]
[0107] (1) The polycarbonate resin, polyurethane resin, and acrylonitrile-butadiene-styrene copolymer are dried at 120° C., 70° C., and 80° C., respectively. After 4 hours, they are cooled and added into a mixer (with a rotation speed of 500 rpm) together with a compatibilizer, a noise reduction agent, and a styrene-acrylonitrile-glycidyl methacrylate copolymer for mixing.
[0108] (2) Add β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate octadecyl ester, bis(2,6-di-tert-butyl-4-methylphenyl) pentaerythritol diphosphate, and pentaerythritol stearate into another mixer (rotating speed is 500 rpm) and mix.
[0109] (3) Pour the mixture obtained in step (1) and step (2) into the same high-speed mixer (rotation speed is 500 rpm) and mix for 10 min.
[0110] (4) adding the mixed material in step (3) into a parallel twin-screw extruder through a feeder, and performing melt extrusion granulation in the parallel twin-screw extruder (eight zones in total), wherein the process parameters include: a temperature of zone 1 of 230° C., a temperature of zone 2 of 240° C., a temperature of zone 3 of 250° C., a temperature of zone 4 of 250° C., a temperature of zone 5 of 250° C., a temperature of zone 6 of 250° C., a temperature of zone 7 of 245° C., a temperature of zone 8 of 245° C., a die head temperature of 260° C., and a screw speed of 500 rpm; the screw shape of the parallel twin-screw extruder is a single-threaded screw, the ratio of screw length L to diameter D (L / D) is 35, and the screw is provided with two meshing block zones and one reverse thread zone.
[0111] Example 7
[0112] A noise reduction polycarbonate composition of this embodiment is prepared from the following raw materials in parts by weight:
[0113]
[0114] The method for preparing the noise reduction polycarbonate composition of this embodiment comprises the following steps:
[0115] (1) The polycarbonate resin, polyurethane resin, and acrylonitrile-butadiene-styrene copolymer are dried at 120° C., 70° C., and 80° C., respectively. After 4 hours, they are cooled and added into a mixer (with a rotation speed of 500 rpm) together with a compatibilizer, a noise reduction agent, and a styrene-acrylonitrile-glycidyl methacrylate copolymer for mixing.
[0116] (2) Add β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate octadecyl ester, bis(2,6-di-tert-butyl-4-methylphenyl) pentaerythritol diphosphate, and pentaerythritol stearate into another mixer (rotating speed is 500 rpm) and mix.
[0117] (3) Pour the mixture obtained in step (1) and step (2) into the same high-speed mixer (rotation speed is 500 rpm) and mix for 10 min.
[0118] (4) adding the mixed material in step (3) into a parallel twin-screw extruder through a feeder, and performing melt extrusion granulation in the parallel twin-screw extruder (eight zones in total), wherein the process parameters include: a temperature of zone 1 of 230° C., a temperature of zone 2 of 240° C., a temperature of zone 3 of 250° C., a temperature of zone 4 of 250° C., a temperature of zone 5 of 250° C., a temperature of zone 6 of 250° C., a temperature of zone 7 of 245° C., a temperature of zone 8 of 245° C., a die head temperature of 260° C., and a screw speed of 500 rpm; the screw shape of the parallel twin-screw extruder is a single-threaded screw, the ratio of screw length L to diameter D (L / D) is 35, and the screw is provided with two meshing block zones and one reverse thread zone.
[0119] Example 8
[0120] A noise reduction polycarbonate composition of this embodiment is prepared from the following raw materials in parts by weight:
[0121]
[0122] The method for preparing the noise reduction polycarbonate composition of this embodiment comprises the following steps:
[0123] (1) The polycarbonate resin, polyurethane resin, and acrylonitrile-butadiene-styrene copolymer are dried at 120° C., 70° C., and 80° C., respectively. After 4 hours, they are cooled and added into a mixer (with a rotation speed of 500 rpm) together with a compatibilizer, a noise reduction agent, and a styrene-acrylonitrile-glycidyl methacrylate copolymer for mixing.
[0124] (2) Add β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate octadecyl ester, bis(2,6-di-tert-butyl-4-methylphenyl) pentaerythritol diphosphate, and pentaerythritol stearate into another mixer (rotating speed is 500 rpm) and mix.
[0125] (3) Pour the mixture obtained in step (1) and step (2) into the same high-speed mixer (rotation speed is 500 rpm) and mix for 10 min.
[0126] (4) adding the mixed material in step (3) into a parallel twin-screw extruder through a feeder, and performing melt extrusion granulation in the parallel twin-screw extruder (eight zones in total), wherein the process parameters include: a temperature of 230° C. in zone 1, a temperature of 240° C. in zone 2, a temperature of 250° C. in zone 3, a temperature of 250° C. in zone 4, a temperature of 250° C. in zone 5, a temperature of 250° C. in zone 6, a temperature of 245° C. in zone 7, a temperature of 245° C. in zone 8, a die head temperature of 260° C., and a screw speed of 500 rpm; the screw shape of the parallel twin-screw extruder is a double-threaded screw, the ratio of screw length L to diameter D (L / D) is 50, and the screw is provided with two meshing block zones and one reverse thread zone.
[0127] Comparative Example 1
[0128] A noise reduction polycarbonate composition of this embodiment is prepared from the following raw materials in parts by weight:
[0129]
[0130] The method for preparing the noise reduction polycarbonate composition of this embodiment comprises the following steps:
[0131] (1) The polycarbonate resin, polyurethane resin, and acrylonitrile-butadiene-styrene copolymer are dried at 120° C., 70° C., and 80° C., respectively. After 4 hours, they are cooled and added into a mixer (with a rotation speed of 500 rpm) together with a compatibilizer, a noise reduction agent, and a styrene-acrylonitrile-glycidyl methacrylate copolymer for mixing.
[0132] (2) Add β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate octadecyl ester, bis(2,6-di-tert-butyl-4-methylphenyl) pentaerythritol diphosphate, and pentaerythritol stearate into another mixer (rotating speed is 500 rpm) and mix.
[0133] (3) Pour the mixture obtained in step (1) and step (2) into the same high-speed mixer (rotation speed is 500 rpm) and mix for 10 min.
[0134] (4) adding the mixed material in step (3) into a parallel twin-screw extruder through a feeder, and performing melt extrusion granulation in the parallel twin-screw extruder (eight zones in total), wherein the process parameters include: a temperature of zone 1 of 230° C., a temperature of zone 2 of 240° C., a temperature of zone 3 of 250° C., a temperature of zone 4 of 250° C., a temperature of zone 5 of 250° C., a temperature of zone 6 of 250° C., a temperature of zone 7 of 245° C., a temperature of zone 8 of 245° C., a die head temperature of 260° C., and a screw speed of 500 rpm; the screw shape of the parallel twin-screw extruder is a single-threaded screw, the ratio of screw length L to diameter D (L / D) is 35, and the screw is provided with two meshing block zones and one reverse thread zone.
[0135] Comparative Example 2
[0136] A noise reduction polycarbonate composition of this embodiment is prepared from the following raw materials in parts by weight:
[0137]
[0138] The method for preparing the noise reduction polycarbonate composition of this embodiment comprises the following steps:
[0139] (1) The polycarbonate resin, polyurethane resin, and acrylonitrile-butadiene-styrene copolymer are dried at 120° C., 70° C., and 80° C., respectively. After 4 hours, they are cooled and added into a mixer (with a rotation speed of 500 rpm) together with a compatibilizer, a noise reduction agent, and a styrene-acrylonitrile-glycidyl methacrylate copolymer for mixing.
[0140] (2) Add β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate octadecyl ester, bis(2,6-di-tert-butyl-4-methylphenyl) pentaerythritol diphosphate, and pentaerythritol stearate into another mixer (rotating speed is 500 rpm) and mix.
[0141] (3) Pour the mixture obtained in step (1) and step (2) into the same high-speed mixer (rotation speed is 500 rpm) and mix for 10 min.
[0142] (4) adding the mixed material in step (3) into a parallel twin-screw extruder through a feeder, and performing melt extrusion granulation in the parallel twin-screw extruder (eight zones in total), wherein the process parameters include: a temperature of zone 1 of 230° C., a temperature of zone 2 of 240° C., a temperature of zone 3 of 250° C., a temperature of zone 4 of 250° C., a temperature of zone 5 of 250° C., a temperature of zone 6 of 250° C., a temperature of zone 7 of 245° C., a temperature of zone 8 of 245° C., a die head temperature of 260° C., and a screw speed of 500 rpm; the screw shape of the parallel twin-screw extruder is a single-threaded screw, the ratio of screw length L to diameter D (L / D) is 35, and the screw is provided with two meshing block zones and one reverse thread zone.
[0143] Comparative Example 3
[0144] A noise reduction polycarbonate composition of this embodiment is prepared from the following raw materials in parts by weight:
[0145]
[0146] The method for preparing the noise reduction polycarbonate composition of this embodiment comprises the following steps:
[0147] (1) The polycarbonate resin, polyurethane resin, and acrylonitrile-butadiene-styrene copolymer are dried at 120° C., 70° C., and 80° C., respectively. After 4 hours, they are cooled and added into a mixer (with a rotation speed of 500 rpm) together with a compatibilizer, a noise reduction agent, and a styrene-acrylonitrile-glycidyl methacrylate copolymer for mixing.
[0148] (2) Add β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate octadecyl ester, bis(2,6-di-tert-butyl-4-methylphenyl) pentaerythritol diphosphate, and pentaerythritol stearate into another mixer (rotating speed is 500 rpm) and mix.
[0149] (3) Pour the mixture obtained in step (1) and step (2) into the same high-speed mixer (rotation speed is 500 rpm) and mix for 10 min.
[0150] (4) adding the mixed material in step (3) into a parallel twin-screw extruder through a feeder, and performing melt extrusion granulation in the parallel twin-screw extruder (eight zones in total), wherein the process parameters include: a temperature of zone 1 of 230° C., a temperature of zone 2 of 240° C., a temperature of zone 3 of 250° C., a temperature of zone 4 of 250° C., a temperature of zone 5 of 250° C., a temperature of zone 6 of 250° C., a temperature of zone 7 of 245° C., a temperature of zone 8 of 245° C., a die head temperature of 260° C., and a screw speed of 500 rpm; the screw shape of the parallel twin-screw extruder is a single-threaded screw, the ratio of screw length L to diameter D (L / D) is 35, and the screw is provided with two meshing block zones and one reverse thread zone.
[0151] Comparative Example 4
[0152] A noise reduction polycarbonate composition of this embodiment is prepared from the following raw materials in parts by weight:
[0153]
[0154] The method for preparing the noise reduction polycarbonate composition of this embodiment comprises the following steps:
[0155] (1) The polycarbonate resin, polyurethane resin, and acrylonitrile-butadiene-styrene copolymer are dried at 120° C., 70° C., and 80° C., respectively. After 4 hours, they are cooled and added into a mixer (with a rotation speed of 500 rpm) together with a compatibilizer, a noise reduction agent, and a styrene-acrylonitrile-glycidyl methacrylate copolymer for mixing.
[0156] (2) Add β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate octadecyl ester, bis(2,6-di-tert-butyl-4-methylphenyl) pentaerythritol diphosphate, and pentaerythritol stearate into another mixer (rotating speed is 500 rpm) and mix.
[0157] (3) Pour the mixture obtained in step (1) and step (2) into the same high-speed mixer (rotation speed is 500 rpm) and mix for 10 min.
[0158] (4) adding the mixed material in step (3) into a parallel twin-screw extruder through a feeder, and performing melt extrusion granulation in the parallel twin-screw extruder (eight zones in total), wherein the process parameters include: a temperature of zone 1 of 230° C., a temperature of zone 2 of 240° C., a temperature of zone 3 of 250° C., a temperature of zone 4 of 250° C., a temperature of zone 5 of 250° C., a temperature of zone 6 of 250° C., a temperature of zone 7 of 245° C., a temperature of zone 8 of 245° C., a die head temperature of 260° C., and a screw speed of 500 rpm; the screw shape of the parallel twin-screw extruder is a single-threaded screw, the ratio of screw length L to diameter D (L / D) is 35, and the screw is provided with two meshing block zones and one reverse thread zone.
[0159] Comparative Example 5
[0160] A noise reduction polycarbonate composition of this embodiment is prepared from the following raw materials in parts by weight:
[0161]
[0162]
[0163] The method for preparing the noise reduction polycarbonate composition of this embodiment comprises the following steps:
[0164] (1) The polycarbonate resin, polyurethane resin, and acrylonitrile-butadiene-styrene copolymer are dried at 120° C., 70° C., and 80° C., respectively. After 4 hours, they are cooled and added into a mixer (with a rotation speed of 500 rpm) together with a compatibilizer, a noise reduction agent, and a styrene-acrylonitrile-glycidyl methacrylate copolymer for mixing.
[0165] (2) Add β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate octadecyl ester, bis(2,6-di-tert-butyl-4-methylphenyl) pentaerythritol diphosphate, and pentaerythritol stearate into another mixer (rotating speed is 500 rpm) and mix.
[0166] (3) Pour the mixture obtained in step (1) and step (2) into the same high-speed mixer (rotation speed is 500 rpm) and mix for 10 min.
[0167] (4) adding the mixed material in step (3) into a parallel twin-screw extruder through a feeder, and performing melt extrusion granulation in the parallel twin-screw extruder (eight zones in total), wherein the process parameters include: a temperature of zone 1 of 230° C., a temperature of zone 2 of 240° C., a temperature of zone 3 of 250° C., a temperature of zone 4 of 250° C., a temperature of zone 5 of 250° C., a temperature of zone 6 of 250° C., a temperature of zone 7 of 245° C., a temperature of zone 8 of 245° C., a die head temperature of 260° C., and a screw speed of 500 rpm; the screw shape of the parallel twin-screw extruder is a single-threaded screw, the ratio of screw length L to diameter D (L / D) is 35, and the screw is provided with two meshing block zones and one reverse thread zone.
[0168] Table 1 List of main raw materials by weight in the examples and comparative examples
[0169]
[0170]
[0171] Note: (a) Screw structure changes; PC is polycarbonate resin; ABS is acrylonitrile-butadiene-styrene copolymer; TPU is polyurethane resin; EM-500 is a compatibilizer; GM-100 is a noise reduction additive; SAG-001 is styrene-acrylonitrile-glycidyl methacrylate copolymer.
[0172] The polycarbonate compositions prepared in the above examples and comparative examples were subjected to the following performance tests:
[0173] Noise reduction performance: Each sample was made into a 200*200*200 square open box, placed vertically on a fixture, and a 200g steel ball was used to hit the bottom of the box with free fall from 1m vertically above. The noise reduction effect of the material was determined by testing the sound intensity below with a decibel tester placed inside the box. The smaller the value, the better.
[0174] Melt index: tested according to GB / T 3682-2000 standard, the test temperature is 260℃, the load is 5kg.
[0175] Impact performance: tested according to GB / T 1843-2008 standard, the specimen thickness is 4mm, the higher the value, the better.
[0176] Heat deformation temperature: tested according to GB / T 1634-2004 standard, the specimen thickness is 4mm, the load is 0.45Mpa, the higher the value, the better.
[0177] The performance test results are shown in Table 2.
[0178] Table 2 Performance of polycarbonate compositions of Examples and Comparative Examples
[0179]
[0180]
[0181] Examples 1 to 7 are polycarbonate compositions prepared by adjusting the addition amounts of polycarbonate, polyurethane resin, acrylonitrile-butadiene-styrene copolymer, compatibilizer, and styrene-glycidyl methacrylate copolymer.
[0182] In the raw materials for preparing the polycarbonate composition of the present invention, the noise reduction system is a compound of low damping materials MDI and TDI copolymer polyurethane and silicone masterbatch, wherein the weight parts of MDI and TDI copolymer polyurethane are 20 to 35 parts, and the weight parts of silicone masterbatch are 1.2 to 1.5 parts; based on the application scenario of the material for automobile interior and exterior plastic parts, the formula system is based on the PC / ABS system. When the proportion of PC / ABS in the formula is high and the proportion of TPU is low, although the noise reduction is improved to a certain extent compared with the pure PC / ABS system, the improvement effect is limited. However, when the proportion of TPU content in the formula reaches a maximum value, the noise reduction effect also reaches a maximum value. However, at this time, due to the poor heat resistance of the TPU resin itself, excessive TPU will cause the stratification of the PC / ABS material, which will cause the impact strength and heat deformation temperature of the modified polycarbonate composition to be too low (such as Examples 1 to 4). When the low damping material MDI and TDI copolymer polyurethane and silicone masterbatch are added in appropriate amounts and work through different pathways, the noise reduction effect on the polycarbonate composition is further improved, and the noise decibel can reach 8. This shows that although the noise reduction mechanisms of the low damping material MDI and TDI copolymer polyurethane and silicone masterbatch in the polycarbonate composition are different, they can be superimposed to enhance the noise reduction effect of the material. When the addition amounts of MDI and TDI copolymer polyurethane and silicone masterbatch are 25 parts and 1.5 parts respectively, the noise reduction effect of the polycarbonate composition reaches an excellent value, and the toughness and processability of the material are also excellent at this time.
[0183] The greater the content of ABS material in the formula, the greater the melt index of the polycarbonate composition, but the lower the impact strength of the polycarbonate polymer. At the same time, the noise reduction performance of the composition will be reduced due to the increase in the amount of TPU added, and reducing the polycarbonate content will further reduce the heat resistance of the material. However, when the content of ABS material in the formula gradually decreases, the melt index of the material gradually decreases, resulting in problems in the production and use of the material, especially in large-size products such as automotive interiors, which are difficult to injection mold, thus limiting the use of polycarbonate compositions. This is mainly because ABS itself has a low molecular weight. Although its heat resistance and noise reduction effects are not outstanding, it has a unique advantage in processability.
[0184] By comparing the various performance data of the polycarbonate compositions prepared in Examples 1 to 7, it is found that under the comprehensive effect of various factors, the polycarbonate composition prepared in Example 7 has the best comprehensive performance and the best ratio of various raw materials.
[0185] Compared with Example 8, the screw shape of the parallel twin-screw extruder used in Example 8 is a double-thread, and the ratio of the screw length L to the diameter D (L / D) is 50. The screw shape of the parallel twin-screw extruder used in Example 7 is a single-thread, and the ratio of the screw length L to the diameter D (L / D) is 35. By comparison, it can be found that the polycarbonate composition prepared by using the screw parameters of the parallel twin-screw extruder described in Example 7 has better impact resistance and processability.
[0186] Compared with Example 7, Comparative Example 1 does not add TPU, but only adds a traditional PC / ABS alloy with a noise reduction additive. The heat resistance of the obtained polycarbonate composition is relatively excellent, but the melt flow rate, impact strength, and noise reduction performance are all worse than those of Comparative Example 1. This is because the heat resistance of the TPU resin itself is worse than that of the ABS resin. Its introduction reduces the overall heat deformation temperature of the material, but the TPU resin itself has excellent processability and for the PC / ABS system, the addition of an appropriate amount of TPU can have a toughening effect, so that the overall macroscopic performance of the material is reduced temperature resistance, and increased melt flow rate and impact strength.
[0187] Compared with Example 7, Comparative Example 2 is a PC / TPU alloy without adding ABS resin. The noise reduction effect of the obtained polycarbonate composition is significantly enhanced, but the overall temperature resistance of the material is lower, and the impact strength of the material is significantly reduced due to the introduction of excessive TPU resin. In addition, due to the poorer compatibility between PC and TPU resins, the particles obtained by granulation are obviously stratified, which shows that the addition of ABS resin can not only improve the overall fluidity of the material, but also play a coordinating role between PC and TPU resins. The three resins coexist, thereby balancing the overall performance of the polycarbonate composition.
[0188] Compared with Example 7, in Comparative Example 3, no compatibilizer EM-500 was added, and the impact strength of the obtained polycarbonate composition decreased significantly, which shows that the compatibilizer is indispensable for improving the compatibility and impact strength of each item in the polycarbonate composition.
[0189] Compared with Comparative Example 3, in Comparative Example 4, more noise reduction agent GM-100 was added, and the various properties of the polycarbonate composition obtained did not change significantly, especially the noise reduction performance did not improve with the addition of GM-100. Moreover, since silicone masterbatch is also a kind of external lubricant, excessive addition will cause the material to slip during the injection molding process, causing the injection molding machine screw to make production difficult.
[0190] Compared with Example 7, in Comparative Example 5, styrene-acrylonitrile-glycidyl methacrylate copolymer SAG-001 was not added, and the impact strength and melt index of the obtained polycarbonate composition were slightly reduced, and the noise reduction performance of the material did not change, indicating that SAG-001 has a significant effect in improving the compatibility of the polycarbonate composition, thereby achieving the purpose of improving the comprehensive performance of the material.
[0191] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0192] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A noise reducing polycarbonate composition, characterized in that: It is prepared from the following raw materials in parts by weight: 40-70 parts of polycarbonate resin, 20-30 parts of polyurethane resin, 10 to 25 parts of acrylonitrile-butadiene-styrene copolymer, 4 to 8 parts of compatibilizer, 1.2-1.5 parts of noise reduction agent, 0.5 to 2 parts of styrene-acrylonitrile-glycidyl methacrylate copolymer, Hindered phenol antioxidant 0.1-0.3 parts, 0.1-0.5 parts of phosphite antioxidant, Pentaerythritol stearate 0.2-0.5 parts, Wherein, the total weight of the polycarbonate resin, the polyurethane resin and the acrylonitrile-butadiene-styrene copolymer is 100 parts; The noise reduction agent is a silicone masterbatch, and the polyurethane resin is a copolymerized polyurethane of TDI and MDI; The compatibilizer is a terpolymer of methyl methacrylate-butadiene-styrene; The mass fraction of glycidyl methacrylate in the styrene-acrylonitrile-glycidyl methacrylate copolymer is 2-4wt%.
2. A noise reduction polycarbonate composition according to claim 1, characterized in that: It is prepared from the following raw materials in parts by weight: 50-60 parts of polycarbonate resin, 20-30 parts of polyurethane resin, 10 to 20 parts of acrylonitrile-butadiene-styrene copolymer, 4 to 8 parts of compatibilizer, 1.5 parts of noise reduction agent, 0.5 to 2 parts of styrene-acrylonitrile-glycidyl methacrylate copolymer, Hindered phenol antioxidant 0.1-0.3 parts, 0.1-0.5 parts of phosphite antioxidant, Pentaerythritol stearate 0.2-0.5 parts.
3. The noise reducing polycarbonate composition according to claim 1, characterized in that: The polycarbonate resin is bisphenol A polycarbonate, and its melt index is 10-12 g / 10 min under the condition of 300° C. / 1.2 kg.
4. The noise reducing polycarbonate composition according to claim 1, characterized in that: The hindered phenol antioxidant is β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate octadecyl ester; The phosphite antioxidant is bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphate.
5. The method for preparing the noise reducing polycarbonate composition according to any one of claims 1 to 4, characterized in that: The following steps are involved: (1) mixing the dried polycarbonate resin, polyurethane resin, acrylonitrile-butadiene-styrene copolymer, a compatibilizer, a noise reduction agent, and styrene-acrylonitrile-glycidyl methacrylate copolymer to obtain a mixture A; (2) mixing a hindered phenol antioxidant, a phosphite antioxidant and pentaerythritol stearate to obtain a mixture B; (3) Mixing mixture A and mixture B again to obtain mixture C; (4) The mixture C is fed into a parallel twin-screw extruder via a feeder, and melt-extruded and granulated to obtain a noise-reducing polycarbonate composition.
6. The preparation method according to claim 5, characterized in that: The temperature of the first zone of the parallel twin-screw extruder is 210-240°C, the temperature of the second zone is 230-260°C, the temperature of the third zone is 235-260°C, the temperature of the fourth zone is 220-260°C, the temperature of the fifth zone is 220-260°C, the temperature of the sixth zone is 220-260°C, the temperature of the seventh zone is 220-260°C, the temperature of the eighth zone is 220-260°C, the die head temperature is 240-275°C, and the screw speed is 200-600rpm; The screw shape of the parallel twin-screw extruder is a single-thread, and the length-to-diameter ratio L / D of the screw is 35-50; the screw is provided with more than one meshing block area and more than one reverse thread area.
7. The preparation method according to claim 5, characterized in that: The drying temperature in step (1) is 80-110° C. and the drying time is 4-8 hours; the mixing stirring speed is 400-600 rpm.
8. The preparation method according to claim 5, characterized in that: The stirring speed of the mixing in step (2) is 400 to 600 rpm; The mixing in step (3) is performed at a stirring speed of 400 to 600 rpm and a stirring time of 8 to 12 min.