A kind of thermoplastic polyurethane elastomer and preparation method thereof

By using a chain extender with a long carbon side chain with a carboxylate ester during the processing of the TPU, the processing temperature of the TPU is reduced and the additive migration is avoided, which solves the problem of degradation of thermoplastic polyurethane elastomers at high temperatures and additive migration. , improves printing performance and material durability.

CN116589655BActive Publication Date: 2024-11-26MEISHAN UBERUI SPECIAL NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310743022.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-21
Publication Date
2024-11-26
Estimated Expiration
2043-06-21

AI Technical Summary

Technical Problem

The existing thermoplastic polyurethane elastomers are relatively high during processing and are prone to thermal degradation. Adding additives requires the reduction of viscosity, but the additives are easy to migrate, affecting the performance of the material.

Method used

A chain extender with carboxylic acid ester long carbon side chain or metadiol is used to reduce the processing temperature of the TPU by plasticizing in a twin-screw reactor, and avoid the use of lubricating additives to reduce the migration of additives.

Benefits of technology

It significantly reduces the processing temperature of the TPU, reduces thermal degradation, improves the printing performance and durability of the material, while avoiding additive migration, and improving the safety and performance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116589655B_ABST
    Figure CN116589655B_ABST
Patent Text Reader

Abstract

The present invention provides a thermoplastic polyurethane elastomer and a preparation method thereof, belonging to the technical field of polyurethane preparation. The preparation method of the thermoplastic polyurethane elastomer comprises the following steps: (1) heating a polymer diol to 60-110°C; (2) heating a diisocyanate to 40-80°C; (3) heating a chain extender to 45-80°C, wherein the molecular formula of the chain extender is at least one of the formulas <Ⅰ>, <Ⅱ>, and <Ⅲ>; wherein R1 is a straight chain or branched chain alkyl group of C4-C20; (4) mixing the heated materials and injecting them into a twin-screw reactor for reaction plasticization, and obtaining a thermoplastic polyurethane elastomer after extrusion. The addition of the chain extender in the present invention can provide lubrication of the molecular chain, reduce the interaction force between the molecular chains, thereby reducing the subsequent processing temperature of TPU and reducing the degradation of TPU. In addition, the lubricating effect of the chain extender can avoid the addition of lubricating additives during the processing of TPU, fundamentally solving the problem of easy migration of lubricating additives. #imgabs0#
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polyurethane processing, and specifically relates to a thermoplastic polyurethane elastomer and a preparation method thereof. Background Art

[0002] Thermoplastic polyurethane elastomer (TPU) is a general term for a class of thermoplastic elastomers containing urethane bonds, which are generally synthesized from macromolecular polyols, small molecule chain extenders and isocyanates. The molecular chain of TPU is basically linear, with a certain amount or a small amount of physical crosslinking. [1-2] Due to its excellent wear resistance, good elasticity and environmental protection performance, it has been widely used in aerospace, automobile manufacturing, medical equipment and other fields. [3] .

[0003] TPU materials have been considered to be difficult to mold thermoplastic elastomers due to their poor flow properties and strong adhesion to processing and molding equipment. Due to the special internal structure of TPU, its macromolecular chain is a pure linear structure, which can be mainly processed and molded by the melt method or solution method. The melt method is currently the most commonly used polyurethane elastomer processing method, and the melt processing methods include calendering, extrusion, blow molding and molding. The advantages of the melt method are: high production efficiency, less time consumption, good appearance of the finished product, and waste products can be reused; fillers such as masterbatch and plasticizer can also be added during the injection molding and extrusion process. The disadvantages of the melt method are: the mold is expensive, the surface is easy to wear, and regular grinding and polishing maintenance are required; it is only suitable for molding small products, not large products. Solution processing mainly dissolves solid TPU in a solvent, and uses the solution for spinning and coating. The advantages of the solution method are: the reaction is slow and easy to control; the disadvantage is: in order to avoid side reactions, the solvent must have a relatively high purity [4] .

[0004] For TPU products with general regular structures, injection molding, blow molding and 3D printing are usually used for production. For TPU products with large hollow curved thin-wall structures and other complex structures, due to the complex structure, it is difficult to obtain products with dimensions and structures that meet the design requirements using traditional molding methods. Dip molding, rotational molding, thermal synthesis and hot pressing molding processes can be used for production.

[0005] Under hot processing conditions, due to the influence of the hot oxygen environment, the relative molecular weight of TPU materials is easily reduced, early yellowing and physical properties are reduced. The occurrence of these phenomena is related to the hot pressing time of TPU materials. The longer the hot pressing time, the more obvious these phenomena are. [5] .

[0006] The injection molding temperature and shear rate of TPU materials during processing will affect its viscosity and ultimately its fluidity, thereby affecting the performance and quality of the material and products. Generally speaking, viscosity is more sensitive to temperature than to shear rate. When the melt temperature is too low, it is not conducive to plasticization processing, resulting in excessively high melt viscosity, making flow and molding more difficult, affecting the re-crystallization of the material after high-temperature melting, thereby affecting the material performance, and the molded products are prone to defects such as weld marks, rough and dull surface, and lack of material; and although a higher melt temperature is helpful for plasticization and reducing viscosity, the method of increasing temperature to reduce viscosity and thus improve fluidity is not a panacea, because although the temperature can be increased a lot, the viscosity decreases only to a limited extent, and at the same time, the heat energy loss increases, and the degradation trend strengthens, which ultimately leads to increased production costs, deterioration of material performance and product quality. [6] .

[0007] In view of the shortcomings of polyurethane elastomers, such as poor high temperature resistance and easy hydrolysis, domestic Liming Chemical Research Institute and other units have improved the performance of polyurethane elastomers by increasing the degree of microphase separation of soft and hard segments, increasing the crosslinking density of elastomer molecules, and selecting raw materials such as isocyanates and chain extenders. In addition, the thermal stability of polyurethane elastomers has been improved by adding fillers, heat stabilizers, antioxidants, etc. [7] .

[0008] Polyurethane elastomers can be widely used in printing, coating and other industries due to their good oil resistance and solvent resistance. In the field of printing, polyurethane elastomers are not only required to have a low hardness, but also to have good solvent resistance. Generally, the synthesis of low-hardness elastomer products is achieved by adding a large amount of plasticizers. Since plasticizers exist in the system by weak intermolecular forces, when the elastomer is soaked in solvent, the plasticizer will precipitate from the system, which will increase the hardness of the elastomer on the one hand, and on the other hand, it will also cause the elastomer to swell and become brittle, affecting its use.

[0009] Therefore, different additives are usually required to be added during the TPU processing and production process. The added additives include: hydrolyzing agents that can inhibit the hydrolysis of TPU, release agents that improve the demolding effect of TPU, plasticizers that reduce hardness, antioxidants that inhibit the oxidative decomposition of TPU, light stabilizers, etc., as well as lubricating additives such as EBS (N,N'-ethylene bisstearamide) and polyethylene wax used to reduce surface adhesion.

[0010] Most additives in the TPU production process are added through mechanical mixing, which is a low-cost and simple process. However, it is necessary to consider the compatibility of the additives with the TPU matrix, the dispersibility of the additives in TPU, and the interface between the additives and TPU. These aspects may cause most additives to volatilize and migrate during the TPU production process, which will seriously affect the appearance and performance of TPU products and have potential impacts on human health and the environment.

[0011] In order to solve the problem of easy migration of additives, the existing methods mainly focus on the following aspects: (1) Through the means of adding additives and in-situ synthesis, the additives are evenly dispersed in the base to achieve migration resistance; (2) Through the means of surface modification, the addition of additives is reduced, thereby preventing the migration of additives; (3) The surface of TPU materials is treated by physical or chemical methods to inhibit the migration of additives.

[0012] Some people add 20-40% plasticizer to thermoplastic polyurethane elastomer with Shore A hardness of 85-90 to prepare soft thermoplastic polyurethane elastomer products with Shore A hardness less than 60. This process can produce products with good crystallization and processing properties, but it also has defects such as migration and exudation of plasticizers and unpleasant odor of products. [8] .

[0013] Patent document CN 110951043 A discloses a method for preparing a highly efficient halogen-free flame-retardant TPU material. The TPU material is prepared by adding an auxiliary agent and synthesizing it in situ, so that the flame retardant has good compatibility and uniform dispersion in the TPU matrix, thereby achieving the characteristic of flame retardant resistance to migration.

[0014] Patent document CN 109679323 A discloses a method for preparing a non-sticky matte soft TPU, which includes adding an anti-sticking agent to the TPU raw material, thereby successfully solving the problem of stickiness on the surface of the matte soft TPU finished product, and avoiding the subsequent migration and precipitation of EBS, polyethylene wax, etc. caused by the conventional use of external slip agents such as EBS, polyethylene wax, etc. to solve the stickiness on the surface of the soft TPU finished product.

[0015] Patent document CN 109679051 A discloses a method for preparing a thermoplastic polyurethane elastomer, which includes adding a bonding agent to the raw material and introducing polar side groups into the TPU hard segment, thereby improving the interaction between the molecular chains of the TPU itself, thereby effectively inhibiting the migration or precipitation of the additive and improving the surface properties of the material.

[0016] Therefore, the existing methods for avoiding the addition of EBS and preventing its migration mainly add other additives to replace the function of EBS. However, such methods still fail to solve the problem of how to avoid using additives, and cannot completely reduce and avoid the addition of additives, and thus fail to fundamentally solve the problem of additive migration, so that the performance of the prepared polyurethane elastomer is greatly affected, such as the printing performance.

[0017] On the other hand, TPU has poor heat resistance. During the thermal processing, due to the strong interaction between the molecular chains, higher temperatures and stronger shearing are often required. TPU is prone to thermal degradation when plasticized at high temperatures, resulting in a decrease in material performance and a reduction in the number of times the material can be recycled.

[0018] High temperature resistant polyurethane elastomer is a popular research direction. There are several ways to solve the heat resistance problem, such as compounding with other materials to change the heat resistance deformation performance, or introducing rigid structures to improve the temperature resistance of the hard segment and soft segment respectively, thereby enhancing the temperature resistance of the material.

[0019] Reports show that by improving the selection and matching of polyurethane raw materials, the heat resistance of polyurethane products can be effectively improved, while maintaining its good processing characteristics and enhancing its hydrolysis resistance. For example, the combination of CHDI and HDI, these aliphatic diisocyanates have significantly improved heat resistance compared to the more common MDI and TDI.

[0020] Patent document CN 108192063 A discloses a high-hardness thermoplastic polyurethane elastomer and its preparation method. The patented method improves the rigidity of the TPU segment by introducing a benzene-ring-containing polyester polyol into the TPU soft segment, thereby significantly reducing the content of the hard segment, reducing the aggregation of the hard segment, effectively reducing the processing temperature of the TPU, and improving the processing performance. When the hardness of the TPU can reach 80D, the patented method can control the processing temperature within 220°C, but its minimum injection molding processing temperature still reaches 190°C.

[0021] Patent document CN 109705302A discloses a method for preparing thermoplastic polyurethane for producing high-resilience and high-brightness foam beads, which comprises mixing and pre-treating the raw material components, and then injecting the pre-treated materials into a twin-screw extruder from a feed port, and injecting phosphite antioxidants, stearates, and butylene terephthalate lubricants into the twin-screw extruder from an exhaust port, thereby achieving extrusion processing at 180-240°C.

[0022] It can be seen from the above literature that the existing methods can solve the high processing temperature of TPU and reduce the processing temperature to a certain extent to prevent thermal degradation of the material. However, the above existing methods still have a high processing temperature of TPU and cannot significantly reduce the processing temperature of TPU, thereby failing to solve the problem of material degradation during thermal processing.

[0023] It can be seen that the existing methods cannot simultaneously achieve the goals of significantly reducing the processing temperature of TPU to prevent its degradation and avoiding the addition of additives to effectively prevent the migration of additives.

[0024] Therefore, how to provide a method for preparing thermoplastic polyurethane so as to significantly reduce the processing temperature of thermoplastic polyurethane and prevent its degradation reaction during thermal processing; on the other hand, to avoid the addition of additives and fundamentally prevent the migration of additives during thermal processing, thereby affecting the performance of polyurethane elastomers, such as improving its printing performance, has become a technical problem that needs to be solved urgently.

[0025] The references cited are as follows:

[0026] [1] Liu Yijun. Polyurethane resin and its application [M]. Beijing: Chemical Industry Press, 2011: 190.

[0027] [2] Liu Houjun. Handbook of Polyurethane Elastomers[M]. Beijing: Chemical Industry Press, 2012: 105-108.

[0028] [3] Yang Wenquan, Qin Xinlin. Research and application of thermoplastic polyurethane elastomer (TPU) [J]. Plastics Manufacturing, 2015(7): 70-77.

[0029] [4] Wei Jian, Master's thesis of Qingdao University of Science and Technology, Synthesis and properties of thermoplastic polyurethane elastomer (TPU)[D], 2021.

[0030] [5] Chen Bingyong, Ding Ning, Liu Jun, et al. Research on hot pressing molding process of TPU materials[J]. Rubber Industry, 2022(005):069.

[0031] [6] Su Lili, Han Bing, Shi Yalin. Effects of injection molding conditions on the properties of thermoplastic polyurethane elastomers [J]. Proceedings of the 2015 Annual Meeting of the Elastomer Professional Committee of China Polyurethane Industry Association, 2015.

[0032] [7] Guo Shanshan, Master's thesis of Qingdao University of Science and Technology, Preparation of MDI system polyurethane elastomer and its dynamic and heat resistance properties[D], 2018.

[0033] [8] Xie Zengwen, Master's thesis of Beijing University of Chemical Technology, Study on the process and properties of thermoplastic polyurethane elastomers produced by twin-screw reactive extrusion[D], 2013. Summary of the invention

[0034] The present invention is to solve the above technical problems, thereby providing a thermoplastic polyurethane elastomer and a preparation method thereof. The technical purpose of the present invention is to solve the problem that the temperature of the existing thermoplastic polyurethane elastomer is high during the processing, and the TPU material is prone to thermal degradation, and provide a method that can significantly reduce the processing temperature of TPU; on the other hand, it solves the problem that the existing TPU needs to add various additives during processing, which easily causes the additives to migrate during thermal processing, seriously affecting the performance of the material, such as poor printing performance.

[0035] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0036] In a first aspect, the present invention provides a method for preparing a thermoplastic polyurethane elastomer, comprising the following steps:

[0037] (1) dehydrating the polymer diol and heating it to 60-110° C.;

[0038] (2) heating the diisocyanate to 40-80° C.;

[0039] (3) heating the chain extender 1 to 45-80° C.; the molecular formula of the chain extender 1 is at least one of the following formulas:

[0040]

[0041] Wherein, the R1 is a C4-C20 straight chain or branched alkyl group;

[0042] (4) The heated materials are mixed and injected into a twin-screw reactor for reaction and plasticization, and the thermoplastic polyurethane elastomer is obtained after extrusion.

[0043] The preparation method of the thermoplastic polyurethane elastomer provided by the present invention uses a chain extender 1 in the chain extension reaction, and the structural formula of the chain extender 1 is at least one of the formulas <Ⅰ>, <Ⅱ>, and <Ⅲ>, which is an ortho- or meta-diol with a carboxylate long carbon side chain, and an ortho-diol containing a long carbon alkyl side chain. The inventor unexpectedly discovered that using the substance with the above structure as a chain extender can provide lubrication for the molecular chain and reduce the force between the molecular chains, thereby reducing the subsequent processing temperature of TPU and reducing the degradation of TPU. On the other hand, the lubrication effect provided by the chain extender can avoid the use of lubricants such as EBS and other various anti-sticking agents, bonding agents and other additives, thereby fundamentally solving the migration problem caused by the need to use a large amount of additives in the existing TPU processing process, and significantly improving the performance of the polyurethane elastomer, for example, its printing performance has been significantly improved.

[0044] As described in the background technology of the present invention, the existing methods can only solve the problem of lowering the processing temperature of TPU or can only solve the problem of preventing the migration of additives, but cannot solve the above two problems at the same time. In addition, the methods of solving the migration of additives in the existing literature often choose to prevent the migration problem of certain lubricating additives such as EBS by adding other additives, but cannot directly avoid the addition of additives, and cannot fundamentally solve the problem of easy migration caused by the use of additives. The method of the present invention uses a chain extender with the above-mentioned structural formula, and only a small amount needs to be added to play a lubricating role between molecular chains, so that TPU can be processed without using a lubricating additive. Therefore, the method of the present invention fundamentally solves the problem of easy migration of added additives, and significantly improves the use performance of this type of polyurethane elastomer, such as the printing performance of the material is significantly improved.

[0045] On the other hand, the method provided by the present invention can significantly reduce the processing temperature of TPU, and can reduce the processing temperature to 150-160°C and still obtain a polyurethane elastomer product with excellent performance by injection molding. The lower processing temperature can well prevent the degradation of TPU and improve the durability of the material.

[0046] Furthermore, the chain extender 1 includes at least one of glyceryl monostearate, glyceryl caprylate, glyceryl caprate, pentaerythritol distearate, and 1,2-alkyl glycol; preferably, the 1,2-alkyl glycol includes at least one of 1,2-dodecyl glycol, 1,2-octanediol, and 1,2-decanediol.

[0047] Furthermore, in terms of weight percentage, the usage ratio of each material is: polymer diol 1-80%, diisocyanate 20-80%, and chain extender 1 0.3-30%.

[0048] Furthermore, the polymer diol includes at least one of polyether diol, copolyether diol, polyester diol, copolyester diol, polyether-polyester diol and polycarbonate diol, and the number average molecular weight of each of the polymer diols is 400-6000.

[0049] Furthermore, the polyether diol includes at least one of polytetramethylene oxide diol, polypropylene oxide diol and polytetramethylene oxide copolyether diol, and the number average molecular weight thereof is 600-3000.

[0050] Furthermore, the polyester diol includes one or more of polyethylene adipate-1,2-propylene glycol ester diol, polyethylene adipate-1,4-butylene glycol ester diol, polyadipate-1,4-butylene glycol ester diol, and polyadipate-1,6-hexanediol ester diol.

[0051] Furthermore, the diisocyanate includes at least one of aliphatic diisocyanate, alicyclic diisocyanate and aromatic diisocyanate.

[0052] Furthermore, the diisocyanate includes at least one of dicyclohexylmethane diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, toluene diisocyanate, ethyl lysine diisocyanate, xylylene diisocyanate, hydrogenated toluene diisocyanate, naphthalene diisocyanate and p-phenylene diisocyanate.

[0053] Furthermore, step (3) further includes adding a chain extender 2, wherein the chain extender 2 is at least one of BDO and HDO. By adding the chain extender 2 to carry out a chain extension reaction, and adding a small amount of the chain extender 1 of the present invention, better lubrication between molecular chains can be achieved, thereby improving the effect of the present invention. As shown in the embodiments of the present invention, when a mixed chain extender is used, the processing temperature of the polyurethane elastomer can be lower, and when it is extruded at as low as 150°C, a polyurethane elastomer with excellent performance can still be obtained well, and the problem of migration of the additive is well solved.

[0054] Furthermore, the extrusion temperature of the twin-screw extruder is 150-160° C. It should be noted that the scheme of the present invention can significantly reduce the processing injection molding temperature, and still well guarantee the performance of the polyurethane elastomer, such as printing performance, but can also achieve good extrusion at a higher temperature.

[0055] In a second aspect, the present invention provides a thermoplastic polyurethane material prepared by the above method.

[0056] Compared with the prior art, the present invention has the following beneficial effects:

[0057] (1) The present invention uses a chain extender 1 to synthesize TPU. The chain extender 1 is an ortho- or meta-diol with a carboxylate long carbon side chain, or an ortho-diol with a long carbon alkyl side chain, which can play a lubricating role between molecular chains and reduce the interaction between molecular chains, thereby significantly reducing the subsequent processing temperature of TPU, significantly reducing the degradation of TPU, and improving the performance of the material;

[0058] (2) The method of the present invention can avoid the addition of a large amount of additives during the TPU processing process, thereby fundamentally solving the problem of easy migration caused by the addition of additives such as EBS or plasticizers, improving the performance of the material, for example, the printing performance is significantly improved, and at the same time has the characteristics of good safety. BRIEF DESCRIPTION OF THE DRAWINGS

[0059] Figure 1 The printing performance of the pipes prepared in Example 2 of the present invention and Comparative Example 2 was examined.

[0060] Figure 2 The printing performance of the tubes prepared in Example 3 of the present invention and Comparative Example 3 was examined. DETAILED DESCRIPTION

[0061] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is described in detail below in conjunction with the embodiments. It is necessary to point out that the following embodiments are only used to explain and illustrate the present invention and are not used to limit the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above invention content still belong to the protection scope of the present invention.

[0062] Example 1

[0063] A method for preparing a thermoplastic polyurethane elastomer comprises the following steps:

[0064] (1) dehydrating polytetramethylene ether glycol (PTMEG, number average molecular weight 1000Da) and heating to 90°C;

[0065] (2) heating diphenylmethane diisocyanate (MDI) to 50° C.

[0066] (3) Chain extender 1 (GM, glyceryl monostearate) and chain extender 2 (BDO, 1,4-butanediol) were mixed and heated to 80°C;

[0067] (4) The heated materials are mixed and injected into a twin-screw reactor for reaction and plasticization. The extrusion temperature is set at 160° C. After extrusion, the materials are pelletized and dried to obtain the thermoplastic polyurethane elastomer.

[0068] The weight ratio of the above materials is PTMEG:MDI:BDO:GM=60:33:6:1. The structural formula of glyceryl monostearate (GM) is:

[0069]

[0070] Example 2

[0071] A method for preparing a thermoplastic polyurethane elastomer comprises the following steps:

[0072] (1) dehydrating polytetramethylene ether glycol (PTMEG, number average molecular weight 2000Da) and heating to 80°C;

[0073] (2) heating diphenylmethane diisocyanate (MDI) to 45°C;

[0074] (3) Chain extender 1 (PD, pentaerythritol distearate) and chain extender 2 (BDO, 1,4-butanediol) were mixed and heated to 60°C;

[0075] (4) The heated materials are mixed and injected into a twin-screw reactor for reaction and plasticization. The extrusion temperature is set at 155° C. After extrusion, the materials are pelletized and dried to obtain the thermoplastic polyurethane elastomer.

[0076] The weight ratio of the above materials is PTMEG:MDI:BDO:PD=60:32:6:2, and the structural formula of pentaerythritol distearate (PD) is:

[0077]

[0078] Example 3

[0079] A method for preparing a thermoplastic polyurethane elastomer comprises the following steps:

[0080] (1) dehydrating poly(1,4-butylene adipate) (PBA, number average molecular weight 2000 Da) and heating to 100° C.;

[0081] (2) heating isophorone diisocyanate (IPDI) to 60° C.

[0082] (3) Mix chain extender 1 (MNC, capric glyceride) and chain extender 2 (HDO, 1,6-hexanediol) and heat to 45°C;

[0083] (4) The heated materials are mixed and injected into a twin-screw reactor for reaction and plasticization. The extrusion temperature is set at 152° C. After extrusion, the materials are pelletized and dried to obtain the thermoplastic polyurethane elastomer.

[0084] The weight ratio of the above materials is PBA:HMDI:HDO:MNC=60:35:3:2, and the structural formula of capric glyceride (MNC) is:

[0085]

[0086] Example 4

[0087] A method for preparing a thermoplastic polyurethane elastomer comprises the following steps:

[0088] (1) dehydrating poly(1,6-hexanediol adipate) (PHA, number average molecular weight 2000 Da) and heating to 110° C.;

[0089] (2) heating hexamethylene diisocyanate (HDI) to 80° C.

[0090] (3) Chain extender 1 (GMC, glyceryl caprylate) and chain extender 2 (BDO) were mixed and heated to 70°C;

[0091] (4) The heated materials are mixed and injected into a twin-screw reactor for reaction and plasticization. The extrusion temperature is set at 150° C. After extrusion, the materials are pelletized and dried to obtain the thermoplastic polyurethane elastomer.

[0092] The weight ratio of the above materials is PHA:HDI:BDO:GMC=65:30:3:2, and the structural formula of caprylic glyceride (GMC) is:

[0093]

[0094] Example 5

[0095] A method for preparing a thermoplastic polyurethane elastomer, referring to Example 1, except that in step (3), only chain extender 1 is used as the chain extender, and the chain extender 1 is 1,2-dodecyl glycol, and its structural formula is:

[0096]

[0097] Example 6

[0098] A method for preparing a thermoplastic polyurethane elastomer, referring to Example 4, using chain extender 1 and chain extender 2 as mixed chain extenders, and the extrusion temperature is 150° C. The difference is that chain extender 2 is a mixture of BDO and HDO in a mass ratio of 1:1.

[0099] Comparative Example 1

[0100] TPU was prepared according to the method of Example 1, except that:

[0101] The chain extender is only BDO, without GM.

[0102] Comparative Example 2

[0103] TPU was prepared according to the method of Example 3, except that:

[0104] The chain extender is HDO, and no MNC is added.

[0105] Comparative Example 3

[0106] Referring to the method in patent CN109679323 B, the anti-sticking agent therein was added to the formula of Example 1, and the chain extender was selected as BDO only, and the extrusion temperature of the twin-screw reactor was set to 180°C.

[0107] Experimental Example 1

[0108] The TPU prepared in the above examples and comparative examples was tested for performance. The Shore hardness test was carried out in accordance with GB / T531-2009 standard; the mechanical property test was carried out in accordance with GB / T528-2009 standard; the migration resistance test method was: in a constant temperature and humidity chamber, 85°C, 85% humidity, and the precipitation on the surface of the material was observed. The results are shown in Table 1:

[0109] Table 1

[0110]

[0111] Experimental Example 2

[0112] The polyurethane elastomer obtained in the embodiment and the comparative example was used to extrude a pipe, and two pipes with the same Shore hardness were selected. The surfaces of the pipes were printed with ink to examine their printing performance. After the two pipes were wiped with alcohol and printed, they were naturally air-dried for 3 hours, and then wiped with alcohol 5 times to observe their state. Figure 1 (Take Example 2 and Comparative Example 2 as examples, the effects of other embodiments are similar). Figure 1 It can be seen that after wiping, the pattern printed by the product of the embodiment of the present invention is clearer, indicating that no migration occurs and the product has better printing performance.

[0113] Experimental Example 3

[0114] The polyurethane elastomer obtained in the embodiment and the comparative example was used to extrude the pipe. After the extruded pipe was not treated, printing was directly performed on the surface of the pipe. The indoor temperature was 20°C. After one week of printing, the pipe was wiped with alcohol 5 times and its state was observed. Figure 2 (Take Example 3 and Comparative Example 3 as examples). Figure 2 It can be seen that the product prepared in the embodiment of the present invention does not have the phenomenon of plasticizer migration to the surface, the adhesion after printing is better, and the product pattern is clearer.

Claims

1. A method for preparing a thermoplastic polyurethane elastomer, characterized in that: Prepared by the following steps: (1) heating polytetramethylene glycol to 90°C; (2) heating diphenylmethane diisocyanate to 50°C; (3) heating the chain extender to 80° C.; the chain extender is 1,2-dodecyl glycol; (4) Mixing the heated materials and injecting them into a twin-screw reactor for reaction and plasticization, and then extruding them at 160° C. to obtain the thermoplastic polyurethane elastomer; Among them, by weight percentage, the usage of each material is as follows: polytetramethylene ether diol 60%, diphenylmethane diisocyanate 33%, and chain extender 7%.

2. The preparation method according to claim 1, characterized in that: The number average molecular weight of the polytetramethylene ether glycol is 1000 Da.

3. Thermoplastic polyurethane elastomer prepared by the method according to claim 1 or 2.