A Mg-Al-RE-Zn-Ca-Mn rare earth magnesium alloy and preparation method thereof
By introducing multiple rare earth and rare earth-alkali earth elements into magnesium alloys, optimizing component matching and forming specific precipitation phases, the problem of difficulty in taking into account both strength and plasticity in large-sized components is solved, and the mechanical properties of magnesium alloys are significantly improved. It has achieved the expansion of applications in the fields of automobiles and rail transit.
Patent Information
- Application Number
- CN202211577809.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-05
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-12-05
AI Technical Summary
The application of magnesium alloys in automobiles and rail transit fields is limited by strength, plasticity and corrosion resistance. The existing Mg-Al-Mn alloys show low strength and poor fluidity in large-size lightweight components, and require rare earth elements. to improve its comprehensive performance.
Using Mg-Al-RE-Zn-Ca-Mn rare earth magnesium alloy, the composite application of multiple rare earth and rare earth-alkali earth elements is optimized to improve the mechanical properties and process suitability of the alloy. Through La-Sm and Y/Gd The alloying action forms a specific precipitation phase, regulates the microstructure morphology, and enhances the tensile strength, yield strength and elongation of the alloy.
The mechanical properties of magnesium alloys have been improved, with tensile strength, yield strength and elongation reaching 240~260MPa, 175~190MPa, 4~7%, respectively, which is significantly better than traditional commercial AZ91/AM60 alloys, and solves the large size of magnesium alloys. Application problems in components.
Smart Images

Figure BDA0003981411310000071 
Figure BDA0003981411310000072 
Figure BDA0003981411310000081
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of magnesium alloys, and in particular relates to a Mg-Al-RE-Zn-Ca-Mn rare earth magnesium alloy and a preparation method thereof. Background Art
[0002] With the development of technology in the field of automobile manufacturing, the demand for large-sized lightweight components is becoming increasingly urgent, which puts higher requirements on the strength, plasticity and damping performance of magnesium-based lightweight alloys. Mg-Al-Mn alloys represented by AM60 are widely used due to their excellent casting process performance, good plasticity and good shock absorption performance. However, this type of alloy also has inherent performance disadvantages such as low strength and relatively poor fluidity, which limits its further expansion of application. At present, the application of magnesium alloys in the automotive field has expanded from small parts such as shells and covers to large thin-walled complex parts and key load-bearing systems. The above problems are more serious. In order to solve these shortcomings, rare earth elements are introduced into the alloy system in order to improve its strength and corrosion resistance while maintaining the excellent plasticity of this series of alloys, thereby expanding the application field of this series of alloys.
[0003] Rare earth elements have a good strengthening effect in magnesium alloys. The right amount of rare earth elements not only retains the plasticity of Mg-Al alloys, but also improves the strength and corrosion resistance of the alloys. Its comprehensive performance has been significantly improved compared with AZ91 / AM60 magnesium alloys. At present, there are relatively few studies on the optimization of mixed rare earth components and specific combinations in the field of magnesium alloys, and Mg-Al alloys with rare earth additions have not yet shown outstanding mechanical properties. Summary of the invention
[0004] In view of this, an object of the present invention is to provide a Mg-Al-RE-Zn-Ca-Mn rare earth magnesium alloy and a preparation method thereof. The rare earth magnesium alloy provided by the present invention has good comprehensive properties.
[0005] The present invention provides a Mg-Al-RE-Zn-Ca-Mn rare earth magnesium alloy, the composition of which is:
[0006] Al: 4.5~7.5wt%
[0007] La: 1.5-3.0wt%,
[0008] Sm: 0.5~1.0wt%
[0009] RE excluding La and Sm: 0.02-0.10wt%,
[0010] Zn: 0.6~1.0wt%
[0011] Ca: 0.15~0.50wt%
[0012] Mn: 0.20~0.40wt%
[0013] The balance is Mg and inevitable impurities.
[0014] Preferably, the ingredients are:
[0015] Al: 5.5~6.5wt%
[0016] La: 2.5-3.0wt%,
[0017] Sm: 0.8~1.0wt%
[0018] RE excluding La and Sm: 0.02-0.05wt%,
[0019] Zn: 0.8~0.9wt%
[0020] Ca: 0.15~0.25wt%
[0021] Mn: 0.25~0.30wt%
[0022] The balance is Mg and inevitable impurities.
[0023] Preferably, the mass ratio of La to Sm is (2.8-3.2):1.
[0024] Preferably, the RE excluding La and Sm is selected from at least one of Y and Gd.
[0025] Preferably, the mass content of the unavoidable impurities is less than 0.2%.
[0026] The present invention provides a method for preparing the Mg-Al-RE-Zn-Ca-Mn rare earth magnesium alloy described in the above technical solution, comprising:
[0027] After melting the Mg ingot and the Al ingot, the temperature is raised once, and then the Mg-La master alloy, the Mg-Sm master alloy, and the Mg-Mn master alloy are added in sequence, and after melting, the master alloy is allowed to stand for a first time to obtain a first melt;
[0028] The temperature of the first melt is maintained at a second temperature, Mg-RE master alloy and Mg-Ca master alloy are added, and after melting, a second standing is performed to obtain a second melt;
[0029] The second melt is heated to a third temperature, degassed and flux is added, and refined, and after the refining is completed, the second melt is cooled to a fourth temperature and subjected to a third standing;
[0030] The alloy liquid after the third standing is deslagging, and then cast at a fifth temperature to obtain a Mg-Al-RE-Zn-Ca-Mn rare earth magnesium alloy.
[0031] Preferably, the temperature of the first heating is 700-730° C.; and the first standing time is 25-35 minutes.
[0032] Preferably, the second temperature is 700-730° C.; and the second standing time is 25-35 min.
[0033] Preferably, the third temperature is 730-750° C.; the fourth temperature is 690-700° C.; and the third standing time is 20-30 min.
[0034] Preferably, the fifth temperature is 680-700°C.
[0035] Aiming at the actual needs of the current automotive, rail transit and other fields, the present invention solves the technical difficulties of poor mechanical properties and difficulty in balancing strength and toughness of magnesium alloys through the composite application of multiple rare earths and rare earth-alkaline earth elements, and effectively improves the mechanical properties and process suitability of the material by constructing an alloy system of Mg-Al-RE-AE with optimized components.
[0036] The present invention is based on the rare earth component matching scheme of the multi-element microalloying effect of rare earth elements. Different rare earth elements will reduce each other's solid solubility in the magnesium alloy, increase the nucleation density and increase the precipitation efficiency under the condition of unchanged total amount, thereby bringing about the effect of improving strength performance and reducing plastic loss. In the present invention, a specific proportion of light rare earth La-Sm with low cost and good processability is selected as the main alloying element, and a specific component matching is formed through the multi-element microalloying effect of a small amount of Y / Gd, which effectively increases the precipitation amount of Al-RE phase, reduces the size of the precipitated phase, and improves the dispersion degree of its distribution.
[0037] The composite application of RE-AE is limited by the nucleation density of the precipitated phase. The Mg-Al / Mg-Al-RE alloy system has no outstanding strengthening effect when the rare earth content is low. By adding an appropriate amount of alkaline earth elements such as Ca, a fine dispersed Al2AE phase can be formed, which is not only a supplement to the Al-RE phase, but also prevents the further growth of the rare earth phase through its dispersed nucleation effect, thereby achieving the effect of refining the microstructure morphology, improving the alloy performance, and reducing the amount of rare earth. However, on the one hand, a low content of Ca elements cannot form an effective improvement effect. On the other hand, too high Ca will gather at the grain boundaries of the microstructure, and Al2Ca particles will also grow rapidly, resulting in a significant reduction in the strength and plasticity of the alloy, and it cannot be used as a main strengthening element. The composite application of rare earth-alkaline earth elements to regulate a variety of Al-RE and Al-AE strengthening phases in the alloy is an effective technical solution to improve the mechanical properties of the alloy chamber.
[0038] After casting, the Mg-Al-RE-Zn-Ca-Mn rare earth magnesium alloy provided by the present invention has a tensile strength, a yield strength and an elongation of 240-260 MPa, 175-190 MPa and 4-7% respectively, and has outstanding advantages in mechanical properties compared with traditional commercial AZ91 / AM60 alloys. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 The microstructure morphology of the cast magnesium alloy prepared in Example 3 of the present invention;
[0040] Figure 2 This is an element distribution analysis of the magnesium alloy microstructure prepared in Example 3 of the present invention. DETAILED DESCRIPTION
[0041] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0042] The present invention provides a Mg-Al-RE-Zn-Ca-Mn rare earth magnesium alloy, the composition of which is:
[0043] Al: 4.5~7.5wt%
[0044] La: 1.5-3.0wt%,
[0045] Sm: 0.5~1.0wt%
[0046] RE excluding La and Sm: 0.02-0.10wt%,
[0047] Zn: 0.6~1.0wt%
[0048] Ca: 0.15~0.50wt%
[0049] Mn: 0.20~0.40wt%
[0050] The balance is Mg and inevitable impurities.
[0051] In the present invention, the mass content of Al is preferably 5-7%, more preferably 5.5-6.5%, and most preferably 6%. Al is a commonly used strengthening element for magnesium alloys, and can form Al-RE and Al-AE precipitation phase particles with RE and AE system elements, thereby effectively improving the material properties. When the aluminum element is less than 4%, the strength of the alloy is improved less and the casting performance is also poor. When the aluminum element is too high, a large amount of Mg 17 Al12 The brittle eutectic phase leads to reduced strengthening effect and decreased alloy plasticity. The aluminum element used in the present invention is in the range of 4.5 to 7.5 wt%.
[0052] In the present invention, the mass content of the La element is preferably 2.0-2.5%, more preferably 2.2-2.3%; the La element has the most obvious precipitation strengthening effect among the light rare earths, and improves the room temperature high temperature mechanical properties of the alloy by forming a high melting point Al-La precipitation phase, but when the La content is too low, there is no outstanding strengthening effect, and when the La content is too high, a large-sized long rod-shaped precipitation phase will be formed, which will split the matrix structure and cause the mechanical properties of the material to decrease. In order to obtain the best strengthening effect, the range of the La element is 2.5-3.0wt%.
[0053] In the present invention, the mass content of the Sm element is preferably 0.6-0.9%, more preferably 0.7-0.8%; the Sm element can prevent the further growth of large-sized Al-La precipitated phases, thereby optimizing the alloy microstructure morphology and improving the material strength and plasticity; but the Al2Sm phase grows rapidly with the increase of Sm content, and absorbs more La elements, affecting the composition ratio of the strengthening phase and weakening the strengthening effect. Therefore, the addition amount of Sm in the present invention has a corresponding proportional relationship with the La element, ranging from 0.8 to 1.0%.
[0054] In the present invention, the RE (rare earth) excluding La and Sm is preferably selected from at least one of Y and Gd; the mass content of the RE excluding La and Sm is preferably 0.03-0.09%, more preferably 0.04-0.08%, more preferably 0.05-0.07%, and most preferably 0.06%; since heavy rare earth elements are preferentially dissolved in the matrix in magnesium, the solid solubility of La / Sm is reduced, the precipitation efficiency is improved, and a better multi-element microalloying strengthening effect is obtained. However, more heavy rare earth will be precipitated and lost in the Mg-Al system, affecting the quality and cost of the alloy. In the present invention, the addition amount of heavy rare earth is 0.02-0.10%.
[0055] In the present invention, the mass content of Zn is preferably 0.7-0.9%, more preferably 0.8%; Zn element has a high solid solubility in magnesium alloys, and can play a strengthening effect in magnesium alloys, which is beneficial to the improvement of the casting performance of magnesium alloys; however, higher Zn is not good for the material's resistance to hot cracking tendency, so a small amount of zinc element is added to the alloy, with a content of 0.6-1.0%.
[0056] In the present invention, the mass content of Ca is preferably 0.20-0.45%, more preferably 0.25-0.40%, and most preferably 0.30-0.35%; the Ca element can promote the refinement of magnesium alloy grains during solidification, and improve the flame retardant properties and fluidity of the alloy by forming a low-viscosity oxide film on the surface of the melt; but too high a calcium content will lead to poor hot cracking performance of magnesium alloy casting and significantly reduce the mechanical properties of the material; the addition range of the calcium element is 0.15-0.50%.
[0057] In the present invention, the mass content of the Mn element is preferably 0.25-0.35%, more preferably 0.30%; the Mn element can play a strengthening effect in the magnesium alloy and promote the formation and dispersion distribution of the Al-RE phase, which is beneficial to the improvement of the casting performance of the magnesium alloy; the addition amount in the present invention is 0.20-0.40%.
[0058] Impurities are inevitable for alloys. In the present invention, the inevitable impurities are selected from Fe, Si, Cu, Ni, etc., and the total impurity mass content is preferably not more than 0.2%.
[0059] In the present invention, the mass ratio of La to Sm is preferably (2.8-3.2):1, more preferably 3:1.
[0060] In the present invention, the composition of the Mg-Al-RE-Zn-Ca-Mn rare earth magnesium alloy is preferably:
[0061] Al: 5.5~6.5wt%
[0062] La: 2.5-3.0wt%,
[0063] Sm: 0.8~1.0wt%
[0064] RE excluding La / Sm: 0.02-0.05wt%,
[0065] Zn: 0.8~0.9wt%
[0066] Ca: 0.15~0.25wt%
[0067] Mn: 0.25~0.30wt%.
[0068] The present invention provides a method for preparing the Mg-Al-RE-Zn-Ca-Mn rare earth magnesium alloy described in the above technical solution, comprising:
[0069] After melting the Mg ingot and the Al ingot, the temperature is raised once, and then the Mg-La master alloy, the Mg-Sm master alloy, and the Mg-Mn master alloy are added in sequence, and after melting, the master alloy is allowed to stand for a first time to obtain a first melt;
[0070] The temperature of the first melt is maintained at a second temperature, Mg-RE master alloy and Mg-Ca master alloy are added, and after melting, a second standing is performed to obtain a second melt;
[0071] The second melt is heated to a third temperature, degassed and flux is added, and refined, and after the refining is completed, the second melt is cooled to a fourth temperature and subjected to a third standing;
[0072] The alloy liquid after the third standing is deslagging, and then cast at a fifth temperature to obtain a Mg-Al-RE-Zn-Ca-Mn rare earth magnesium alloy.
[0073] In the present invention, the first heating is preferably carried out under a protective atmosphere; the temperature of the first heating is preferably 700-730°C, more preferably 715-725°C, and most preferably 720°C; the first standing time is preferably 25-35 min, more preferably 28-32 min, and most preferably 30 min.
[0074] In the present invention, the mass content of La in the Mg-La master alloy is preferably 15-40%, more preferably 20-35%, and most preferably 25-30%; the mass content of Sm in the Mg-Sm master alloy is preferably 15-40%, more preferably 20-35%, and most preferably 25-30%.
[0075] In the present invention, after the melting, it is preferred to stir the mixture thoroughly and evenly before the first standing.
[0076] In the present invention, the second temperature is preferably 700-730°C, more preferably 715-725°C, and most preferably 720°C; the second standing time is preferably 25-35 min, more preferably 28-32 min, and most preferably 30 min.
[0077] In the present invention, the mass content of rare earth in the Mg-RE master alloy is preferably 15-40%, more preferably 20-35%, and most preferably 25-30%.
[0078] In the present invention, the melting is preferably carried out with sufficient stirring and then the second standing is performed.
[0079] In the present invention, the third temperature is preferably 730-750°C, more preferably 735-745°C, and most preferably 740°C; the refining treatment time is preferably 20-35 min, more preferably 25-30 min; the fourth temperature is preferably 690-700°C, more preferably 695°C; the third standing time is preferably 20-30 min, more preferably 25 min.
[0080] In the present invention, the fifth temperature is preferably 680-700°C, more preferably 685-695°C, and most preferably 690°C.
[0081] The present invention has no special limitation on the casting method, and the casting technical solution well known to those skilled in the art can be adopted.
[0082] After the Mg-Al-RE-Zn-Ca-Mn rare earth magnesium alloy provided by the present invention is cast, the tensile strength, yield strength and elongation of the alloy reach 240-260 MPa, 175-190 MPa and 4-7% respectively, and compared with the traditional commercial AZ91 / AM60 alloy, the alloy has outstanding advantages in mechanical properties.
[0083] Embodiment 1 to Embodiment 7
[0084] The rare earth magnesium alloy was prepared according to the following method:
[0085] Under a protective atmosphere, after melting the Mg ingot and the Al ingot, the temperature is raised to 700-730° C., and the Mg-La, Mg-Sm, and Mg-Mn alloys are added in sequence, and after melting, they are fully stirred and allowed to stand for 30 minutes;
[0086] The melt temperature is maintained at 700-730°C, Mg-RE and Mg-Ca alloys are added, and after melting, they are fully stirred and allowed to stand for 30 minutes;
[0087] The melt is heated to 730-750°C, degassed and flux added, and refined for 20-35 minutes. After refining, the melt is cooled to 690-700°C and allowed to stand for 20-30 minutes.
[0088] The slag is removed and cast at a temperature of 680-700°C to obtain a Mg-Al-RE-Zn-Ca-Mn rare earth magnesium alloy.
[0089] Comparative Example 1
[0090] AZ91 magnesium alloy.
[0091] Comparative Example 2
[0092] AM60 magnesium alloy.
[0093] Comparative Example 3 to Comparative Example 7
[0094] A rare earth magnesium alloy was prepared according to the method of the embodiment.
[0095] Performance Testing
[0096] The composition of the rare earth magnesium alloy prepared in the embodiment of the present invention and the comparative example was tested according to the GBT 13748 method. The test results are shown in Table 1 and Table 2:
[0097] Table 1 Composition of rare earth magnesium alloy prepared in Example
[0098]
[0099] Table 2 Composition of rare earth magnesium alloy prepared in comparative example
[0100]
[0101]
[0102] Figure 1 The microstructure of the magnesium alloy cast prepared in Example 3 is as follows: Figure 1 A Optical metallographic structure shows that the alloy microstructure is composed of α-Mg matrix, island or block Al-RE eutectic structure with discontinuous network distribution at grain boundaries; Figure 1 The SEM microstructure of B shows that the eutectic precipitated phase is mainly distributed at the grain boundaries of the matrix. In addition, due to the high contents of Zn and RE, layered LPSO phase can be seen in the grain boundary structure.
[0103] Figure 2 From the element distribution analysis of the magnesium alloy microstructure prepared in Example 3, it can be seen that the main eutectic phase precipitated in the alloy structure is Al-La phase, and there is a common substitution phenomenon of La by Sm element; through the substitution of Sm for La, the long rod-shaped Al-La phase is broken evenly, avoiding the splitting effect of the brittle phase on the matrix, thereby bringing about the improvement effect of multi-rare earth alloying, so that the strength and plasticity of the alloy are improved.
[0104] According to GB / T228.1 "Tensile test of metallic materials Part 1: Room temperature test method", the tensile strength, yield strength and elongation of the rare earth magnesium alloy prepared in the embodiment of the present invention and the comparative example were tested. The test results are shown in Table 3 and Table 4:
[0105] Table 3 Mechanical properties of rare earth magnesium alloys prepared in Example
[0106]
[0107] From the test results in Table 3, it can be seen that the alloys in each embodiment have good strength and plasticity, and the various properties of the alloys prepared in the embodiments of the present invention are most closely related to the Al content and the total amount of rare earth in the alloy. With the increase of rare earth content, the performance increases first and then decreases. When the rare earth content is high, the optimization effect of various properties is significantly weakened. This is because the main strengthening phase Al in the alloy 11The increase in the number of RE3 / Al2RE phases and the change in morphology are the causes. By comparing Examples 1, 5, and 6, it can be seen that when the amount of Ca added is low, the plasticity of the alloy is well improved, but as the Ca content increases, the plasticity of the alloy decreases significantly, and the optimization effect on strength also begins to weaken. The Zn element has a significant effect on the yield strength and plasticity of the alloy. The yield strength increases with the increase of Zn content, and the plasticity of the material decreases with the increase of Zn content.
[0108] Table 4 Mechanical properties of rare earth magnesium alloys prepared in comparative example
[0109]
[0110] It can be seen from the test results of Table 4 that after comparing commercial magnesium alloys (Comparative Example 1, Comparative Example 2) and each major alloying element out of the scope of the present invention, the material properties show significant changes, and compared with the optimized components of the embodiment, the performance has no advantages. After adding rare earth, alkaline earth and other alloying elements, the comprehensive performance of the alloy is better than the currently widely used commercial magnesium alloy. It can be seen from Comparative Examples 1 and 2 that when the content of Al and RE elements is too high, the material causes the microstructure to coarsen and be uneven due to the rapid growth of the precipitated phase, resulting in a rapid decrease in material properties. When the content of Al and RE elements is too low, the number density of the alloy strengthening phase decreases significantly, resulting in insufficient mechanical properties of the alloy, which is lower than that of conventional commercial magnesium alloys. It can be seen from Comparative Examples 3 and 4 that excessive addition of Zn and Ca elements causes the alloy precipitation phase density to be too high, which causes the material plasticity to decrease under the action of the Orwan mechanism, while not adding Zn and Ca elements weakens the precipitation strengthening effect of the alloy, resulting in an insignificant increase in the yield strength of the alloy. It can be seen from Comparative Example 7 that when the rare earth ratio is changed, the La element has a better strengthening effect on strength than the Sm element, but a lower improvement effect on plasticity than the Sm element.
[0111] After pressure casting, the Mg-Al-RE-Zn-Ca-Mn rare earth magnesium alloy provided by the present invention has a tensile strength, a yield strength and an elongation of 240-260 MPa, 175-190 MPa and 4-7% respectively, and has outstanding advantages in mechanical properties compared with traditional commercial AZ91 / AM60 alloys.
[0112] Although the present invention has been described and illustrated with reference to specific embodiments of the present invention, these descriptions and illustrations do not limit the present invention. It will be clearly understood by those skilled in the art that various changes may be made without departing from the true spirit and scope of the present invention as defined by the appended claims, so that specific circumstances, materials, material compositions, materials, methods or processes are suitable for the goals, spirit and scope of the present application. All such modifications are intended to be within the scope of the appended claims. Although the methods disclosed herein have been described with reference to specific operations performed in a specific order, it should be understood that these operations may be combined, subdivided or reordered to form equivalent methods without departing from the teachings of the present invention. Therefore, unless specifically indicated herein, the order and grouping of operations are not limitations of the present application.
Claims
1. A Mg-Al-RE-Zn-Ca-Mn rare earth magnesium alloy, comprising: Al: 4.5wt% or more and less than 7.5wt%, La: 1.5-3.0wt%, Sm: 0.5~1.0wt% The mass ratio of La to Sm is (2.8-3.2):1; RE excluding La and Sm: 0.02-0.10wt%, Zn: 0.6~1.0wt% Ca: 0.15~0.50wt% Mn: 0.20~0.40wt% The balance is Mg and unavoidable impurities; The RE excluding La and Sm is selected from at least one of Y and Gd.
2. The Mg-Al-RE-Zn-Ca-Mn rare earth magnesium alloy according to claim 1, characterized in that: Ingredients: Al: 5.5~6.5wt% La: 2.5-3.0wt%, Sm: 0.8~1.0wt% RE excluding La and Sm: 0.02-0.05wt%, Zn: 0.8~0.9wt% Ca: 0.15~0.25wt% Mn: 0.25~0.30wt% The balance is Mg and inevitable impurities.
3. The Mg-Al-RE-Zn-Ca-Mn rare earth magnesium alloy according to claim 1, characterized in that: The mass content of the unavoidable impurities is less than 0.2%.
4. A method for preparing the Mg-Al-RE-Zn-Ca-Mn rare earth magnesium alloy according to claim 1, comprising: After melting the Mg ingot and the Al ingot, the temperature is raised once, and then the Mg-La master alloy, the Mg-Sm master alloy, and the Mg-Mn master alloy are added in sequence, and after melting, the master alloy is allowed to stand for a first time to obtain a first melt; The temperature of the first melt is maintained at a second temperature, Mg-RE master alloy and Mg-Ca master alloy are added, and after melting, a second standing is performed to obtain a second melt; The second melt is heated to a third temperature, degassed and flux is added, and refined, and after the refining is completed, the second melt is cooled to a fourth temperature and subjected to a third standing; The alloy liquid after the third standing is deslagging, and then cast at a fifth temperature to obtain a Mg-Al-RE-Zn-Ca-Mn rare earth magnesium alloy.
5. The method according to claim 4, characterized in that The temperature of the first heating is 700-730°C.
6. The method according to claim 4, characterized in that The first standing time is 25 to 35 minutes.
7. The method according to claim 4, characterized in that The second temperature is 700-730° C.; the second standing time is 25-35 minutes.
8. The method according to claim 4, characterized in that The third temperature is 730-750° C.; the fourth temperature is 690-700° C.; and the third standing time is 20-30 minutes.
9. The method according to claim 4, characterized in that The fifth temperature is 680-700°C.