A poisoning-resistant organic sulfur hydrogenation catalyst and its preparation and application
The poisoning-resistant organic sulfur hydrogenation catalyst, using ZrO2, Al2O3, and CeO2 with MnO2 and MoO3, addresses the inefficiencies of existing catalysts by achieving high conversion rates of COS and CS2 with reduced energy consumption and side reactions.
Patent Information
- Application Number
- CN202211684511.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-27
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2042-12-27
AI Technical Summary
Existing hydrodesulfurization catalysts suffer from reduced activity and low hydrodesulfurization rates at high temperatures, leading to energy inefficiency and the occurrence of side reactions, particularly in the removal of COS and CS2.
A poisoning-resistant organic sulfur hydrogenation catalyst comprising a carrier made of ZrO2, Al2O3, and CeO2, with active components such as MnO2 and MoO3, or combinations thereof, prepared through a co-precipitation method to enhance catalytic performance and stability.
The catalyst achieves high conversion rates of COS (100%) and CS2 (95%) without side reactions, while maintaining thermal stability and reducing energy consumption, thus offering energy savings and emission reductions.
Smart Images

Figure BDA0004020337580000091 
Figure BDA0004020337580000092 
Figure BDA0004020337580000101
Abstract
Description
Technical Field
[0001] The invention relates to a hydrodesulfurization catalyst, in particular to a poisoning-resistant organic sulfur hydrogenation catalyst and the preparation and application thereof. Background Art
[0002] Hydrogen, methane, carbon monoxide, etc. in coke oven gas, closed furnace, yellow phosphorus tail gas, and blast furnace gas are all recyclable chemicals. However, COS, CS2, H2S, etc. are harmful impurities. These harmful impurities not only pollute the environment, but also corrode equipment, block pipelines, cause catalysts and adsorbents to be poisoned and deactivated, and affect the subsequent recycling process. Therefore, these harmful impurities must be removed before recycling.
[0003] The method to remove these harmful impurities is the waste gas desulfurization technology, which specifically includes wet desulfurization and dry desulfurization. Wet desulfurization can absorb and remove most of the H2S, while organic sulfur such as COS requires dry desulfurization. Commonly used dry desulfurization methods in industry include absorption, pyrolysis, hydrolysis and hydrogenation conversion. The pyrolysis method is greatly affected by the conversion temperature and heat balance and is rarely used. The elemental sulfur and sulfate generated in the hydrolysis method have a great influence on the activity of the catalyst, and may even cause the hydrolysis catalyst to deactivate. In addition, it is difficult for the current high-temperature smelting industrial furnace gas to reach the temperature requirement of less than 100°C for the hydrolysis reaction by cooling. However, the hydrogenation conversion method has a high organic sulfur conversion rate, which converts COS into easily removable H2S, which is then absorbed by an adsorption desulfurizer. And the temperature of the hydrogenation catalyst can reach 200-300°C, which is more energy-efficient than using a hydrolysis catalyst. The principle of removing COS and CS2 by hydrogenation: COS and CS2 react with H2 to generate H2S and CO2 respectively.
[0004] At present, document 1 (patent number CN108940248A) discloses an organic sulfur hydrogenation conversion catalyst and its preparation method and application, which targets organic sulfur components such as COS and C4H4S in coke oven gas. The reaction temperature is 280-360°C, which can inhibit side reactions such as methanation and CO disproportionation during the hydrodesulfurization reaction. However, the reaction temperature of the catalyst is slightly high, the energy consumption is high, and side reactions such as methanation will also occur. There is also document 2 (patent number CN106563475A) that discloses a preparation method for a modified silicon-based catalyst for catalytic hydrolysis of carbonyl sulfide and carbon disulfide. The catalyst has a good removal effect at a relatively low temperature (25°C-60°C), and can achieve the simultaneous removal of carbonyl sulfide and carbon disulfide. However, the reaction temperature of this method is low, and in order to ensure that the hydrolysis catalyst is used without deactivation, a large amount of energy will be lost in cooling. And document 3 (patent number CN101797508A) discloses the preparation of a coke oven gas hydrogenation catalyst, the catalyst is prepared by using γ-Al2O3 as a carrier and loading the active components onto the catalyst carrier by an impregnation method. At 300°C, the hydrogenation desulfurization rate of the catalyst is only about 80%. Summary of the invention
[0005] The purpose of the present invention is to provide a poisoning-resistant organic sulfur hydrogenation catalyst and its preparation and application, which solves the problems of reduced activity and low hydrodesulfurization rate of the catalyst in the prior art in the hydrolysis method at high temperature. The catalytic efficiency is high in the hydrolysis reaction at a temperature of 280°C, the conversion rate of COS is as high as 100%, the conversion rate of CS2 is as high as 95%, no side reactions are generated, and compared with the existing hydrolysis method, it also has the effect of energy saving and emission reduction.
[0006] In order to achieve the above-mentioned purpose, the present invention provides a poisoning-resistant organic sulfur hydrogenation catalyst, which comprises: a carrier and an active component; wherein the carrier is any two or more of ZrO2, Al2O3 and CeO2; the active component is MnO2 and MoO3, or any one or two of MnO2 and MoO3 and Co3O4 and CuO; the mass ratio of the carrier to the active component is (45-85): (15-55).
[0007] Preferably, the mass ratio of the carrier to the active component is 8: 2. Different mass ratios will result in different activities. When the mass ratio of the active component to the carrier is 2: 8, the activity of the catalyst is the best.
[0008] Preferably, the carrier is ZrO2, Al2O3 and CeO2, wherein the mass ratio of ZrO2, Al2O3 and CeO2 is (40-50): (20-30): (20-40). ZrO2 and CeO2 in the carrier both have good redox properties, which are beneficial to improving the catalytic performance of the catalyst, so when the content of ZrO2 and CeO2 is high, the activity of the prepared catalyst is better.
[0009] Preferably, the active components are MnO2 and MoO3, wherein the mass ratio of MnO2 to MoO3 is (4-15): (5-20). When the active components are MnO2 and MoO3, oxidation is favorable and the obtained catalyst has the best activity.
[0010] Preferably, the active components are MoO3, MnO2 and Co3O4, wherein the mass ratio of Co3O4, MnO2 and MoO3 is (8-20): (4-15): (5-20); the active components are MoO3, MnO2 and CuO, wherein the mass ratio of MnO2, MoO3 and CuO is (4-15): (5-20): (10-20); the active components are MoO3, MnO2, Co3O4 and CuO, wherein the mass ratio of Co3O4, MnO2, MoO3 and CuO is (8-20): (4-15): (5-20): (10-20).
[0011] Preferably, the precursors of the active components are soluble salts; and the precursors of the carriers are nitrates.
[0012] The present invention also provides a method for preparing the anti-poisoning organic sulfur hydrogenation catalyst, the method comprising:
[0013] (1) The precursor of the active component and the precursor of the carrier are dissolved, mixed and added with a precipitant, filtered and washed to obtain a precipitate; or the precursor of the carrier is first dissolved, mixed and added with a precipitant, filtered, the filter residue is washed, dried and calcined to obtain a carrier, and then the precursor of the active component is dissolved, mixed and stirred with the obtained carrier, allowed to stand, heated and stirred to obtain a precipitate; (The active component of the co-precipitation method is mainly in the bulk phase, which can increase the synergistic effect between catalysts. The active component of the catalyst of the impregnation method is mainly in the pores and surface. Both methods are conducive to increasing the activity of the catalyst.)
[0014] (2) Drying and calcining the precipitate obtained in step (1) to obtain an anti-poisoning organic sulfur catalyst.
[0015] Preferably, the precursor of the active component is a soluble salt; the precursor of the carrier is a nitrate, wherein the soluble salt is selected from Cu(NO3)2·3H2O, Mn(NO3)2, (NH4)6Mo7O 24 ·4H2O, Co(NO3)2·6H2O or any two thereof; and the nitrate is any two or more of Al(NO3)3·9H2O, Ce(NO3)3·6H2O and Zr(NO3)4·5H2O.
[0016] Preferably, in step (1), the precipitant is sodium carbonate, the drying temperature is 80-100°C, and the calcination temperature is 300-650°C. If the calcination temperature is too high, the catalyst will sinter or agglomerate, and the catalytic activity will decrease; if the temperature is too low, the decomposition temperature of the precursor salt into oxides cannot be reached, and the expected catalyst cannot be obtained. And the slow heating rate of calcination is conducive to the formation of a stable structure of the catalyst, and the prepared catalyst has a good catalytic effect.
[0017] Preferably, in step (1), the heating and stirring are sequentially heated at 40°C, 50°C, 60°C, and 70°C for 1 hour each and continuously stirred. Slow heating helps the active components diffuse into the pores of the carrier, while heating too quickly will easily cause the active components to deposit at the pores, resulting in a decrease in catalyst performance.
[0018] Preferably, in step (2), the drying temperature is 80-100°C.
[0019] Preferably, in step (2), the calcination temperature is 300-700°C.
[0020] Preferably, in step (2), the calcination time is 4 to 6 hours. If the calcination time is too long, the prepared catalyst will be sintered or agglomerated, and if the time is too short, the precursor salt may not be completely decomposed, affecting the performance of the catalyst.
[0021] Preferably, in steps (1) and (2), the heating rate of the calcination is 1 ~ 5℃ / min. The heating rate of the calcination is 1 ~ At 5℃ / min, the structure of the prepared catalyst is stable.
[0022] More preferably, in steps (1) and (2), the heating rate of the calcination is 2° C. / min.
[0023] The present invention also provides an application of the poisoning-resistant organic sulfur hydrogenation catalyst in hydrodesulfurization.
[0024] The poisoning-resistant organic sulfur hydrogenation catalyst of the present invention and its preparation and application solve the problem of reduced activity and low hydrodesulfurization rate of the catalyst in the high-temperature hydrolysis method of the prior art, and have the following advantages:
[0025] 1. The catalyst of the present invention has good thermal stability and long-term effectiveness;
[0026] 2. The catalyst of the present invention not only solves the problem of reduced catalyst activity in the existing hydrolysis reaction at a temperature of 200 to 300° C., but also does not produce side reactions. Compared with the hydrolysis method, the present invention can achieve the effect of energy saving and emission reduction;
[0027] 3. The catalyst of the present invention has high catalytic efficiency and can effectively remove COS and CS2 from sulfides. At 280°C, the conversion rate of COS is as high as 100%, and the conversion rate of CS2 is as high as 95%. DETAILED DESCRIPTION
[0028] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] Example 1
[0030] A method for preparing a poisoning-resistant organic sulfur hydrogenation catalyst, the method comprising:
[0031] (1) 1.5186 g of Cu(NO3)2·3H2O, 3.6777 g of Al(NO3)3·9H2O, 3.4922 g of Ce(NO3)3·6H2O, and 5.2263 g of Zr(NO3)4·5H2O were dissolved in 50 mL of water, mixed, and a precipitant (the precipitant in this embodiment and the following embodiments and comparative examples was a 5% Na2CO3 solution) was added during stirring. 4+ 、Ce 3+ precipitate), add NaOH solution to adjust the pH value to 10-11, then age at 80°C for 6h, filter, and wash with deionized water 2-5 times to obtain a precipitate;
[0032] (2) Add 0.7359 g (NH4)6Mo7O to the precipitate obtained in step (1) 24 After being stirred evenly with 4H2O, the mixture was placed in an oven at 80-100°C and dried overnight to obtain a powder, which was then placed in a muffle furnace at 550°C and kept warm for 4 hours to obtain 5 g of finished catalyst powder.
[0033] Example 2
[0034] A method for preparing a poisoning-resistant organic sulfur hydrogenation catalyst, the method comprising:
[0035] (1) 2.7195 g of Co(NO3)2·6H2O, 5.5166 g of Al(NO3)3·9H2O, and 5.0445 g of Ce(NO3)3·6H2O were dissolved in 50 mL of water, respectively, mixed, and 2 mL of Mn(NO3)2 solution was added, and Na2CO3 precipitation agent was added to precipitate, and NaOH solution was added dropwise to adjust the pH value to 10-11, and then aged at 80°C for 6 h and filtered, and then the precipitate was washed 2-5 times by adding deionized water to obtain a precipitate;
[0036] (2) The precipitate obtained in step (1) is placed in an oven at 80-100° C. and dried overnight to obtain a powder, which is then placed in a muffle furnace and heated to 300° C. at a rate of 2° C. / min and kept warm for 1 h, and then heated to 550° C. at a rate of 2° C. / min and kept warm for 4 h to obtain a finished catalyst powder.
[0037] Example 3
[0038] A method for preparing a poisoning-resistant organic sulfur hydrogenation catalyst, the method comprising:
[0039] (1) 3.7834 g Ce(NO3)3·6H2O, 5.2263 g Zr(NO3)4·5H2O, and 5.5166 g Al(NO3)3·9H2O were dissolved in 50 mL of water, mixed, and 1.3 mL of Mn(NO3)2 solution was added. Na2CO3 precipitant was added during stirring, and NaOH solution was added dropwise to adjust the pH value to 10-11. After aging at 80°C for 6 h, the mixture was filtered and washed with deionized water for 2-5 times to obtain a precipitate.
[0040] (2) The precipitate obtained in step (1) is placed in an oven at 80-100° C. and dried overnight to obtain a powder, which is then placed in a muffle furnace and heated to 300° C. at a rate of 2° C. / min and kept warm for 1 hour, and then heated to 500° C. at a rate of 2° C. / min and kept warm for 4 hours to obtain a finished catalyst powder.
[0041] Example 4
[0042] A method for preparing a poisoning-resistant organic sulfur hydrogenation catalyst, the method comprising:
[0043] (1) 4.5972 g Al(NO3)3·9H2O, 3.7834 g Ce(NO3)3·6H2O, and 7.8394 g Zr(NO3)4·5H2O were dissolved in 50 mL of water, respectively, and mixed. Na2CO3 precipitant was added during stirring, and NaOH solution was added dropwise to adjust the pH value to 10-11. The mixture was aged at 80°C for 6 h, filtered, and washed with deionized water for 2-5 times to obtain a precipitate.
[0044] (2) drying the precipitate obtained in step (1) in an oven at 80-100° C. overnight to obtain a powder, then heating the powder in a muffle furnace at a rate of 2° C. / min to 300° C. and calcining the powder for 1 h, and then heating the powder to 550° C. and calcining the powder for 4 h at a rate of 2° C. / min to obtain a carrier;
[0045] (3) Dissolve 1.813 g of Co(NO3)2·6H2O in 50 mL of water, add 1.3 mL of Mn(NO3)2 solution, add 4 g of the carrier obtained in step (2), stir at room temperature for 2 h, let stand for 1 h, place in a six-hole water bath set to 40°C, 50°C, 60°C, and 70°C, stir continuously for 1 h, dry in an oven overnight, then place in a muffle furnace and heat to 300°C at a rate of 2°C / min and keep warm for 1 h, then heat to 500°C at a rate of 2°C / min and keep warm for 4 h to obtain a finished catalyst.
[0046] Example 5
[0047] The preparation method of a poisoning-resistant organic sulfur hydrogenation catalyst is substantially the same as that of Example 4, except that:
[0048] In step (3), 0.9064 g Co(NO3)2·6H2O, 0.6133 g (NH4)6Mo7O 24 ·4H2O was dissolved in 50mL of water, 1.3mL of Mn(NO3)2 solution was added, and 3.75g of the carrier obtained in step (2) was added. The finished catalyst was obtained by the same operation as step (3) of Example 4.
[0049] Example 6
[0050] The preparation method of a poisoning-resistant organic sulfur hydrogenation catalyst is substantially the same as that of Example 4, except that:
[0051] (1) The masses of Al(NO3)3·9H2O, Ce(NO3)3·6H2O, and Zr(NO3)4·5H2O were 5.5166 g, 3.7834 g, and 6.9683 g, respectively, and the subsequent operation was the same as step (1) of Example 4;
[0052] (2) The carrier is obtained by the same operation as step (2) of Example 4;
[0053] (3) 0.9199 g (NH4)6Mo7O 24 ·4H2O was dissolved in 50 mL of water, 4.25 g of the carrier obtained in step (2) was added, and the finished catalyst was obtained by the same operation as step (3) of Example 4.
[0054] Example 7
[0055] The preparation method of a poisoning-resistant organic sulfur hydrogenation catalyst is substantially the same as that of Example 3, except that:
[0056] In step (1), the mass of Al(NO3)3·9H2O is changed to 3.6777 g;
[0057] In step (2), 0.6132 g (NH4)6Mo7O is added to the precipitate obtained in step (1). 24 ·4H2O, stir evenly, place in an oven at 80-100°C and dry overnight to obtain dry powder, and then perform the same operation as step (2) of Example 3 to obtain the finished catalyst.
[0058] Example 8
[0059] The preparation method of a poisoning-resistant organic sulfur hydrogenation catalyst is substantially the same as that of Example 6, except that:
[0060] In step (3), (NH4)6Mo7O 24 The mass of 4H2O is 0.6133 g.
[0061] Example 9
[0062] A method for preparing a poisoning-resistant organic sulfur hydrogenation catalyst, which is substantially the same as Example 7, except that:
[0063] In step (1), 3.7834 g Ce(NO3)3·6H2O, 7.8394 g Zr(NO3)4·5H2O, and 1.5186 g Cu(NO3)2·3H2O are dissolved in 50 mL of water, mixed, and 0.67 mL of Mn(NO3)2 solution is added. Na2CO3 precipitant is added during stirring, and NaOH solution is added dropwise to adjust the pH value to 10-11. The mixture is then aged at 80°C for 6 h, filtered, and washed with deionized water for 2-5 times to obtain a precipitate.
[0064] Example 10
[0065] The preparation method of a poisoning-resistant organic sulfur hydrogenation catalyst is substantially the same as that of Example 4, except that:
[0066] In step (3), 1.5186 g of Cu(NO3)2·3H2O was dissolved in 50 mL of water, 0.67 mL of Mn(NO3)2 solution was added, and 4.25 g of the carrier obtained in step (2) was added. The finished catalyst was obtained by the same subsequent operation as step (3) of Example 4.
[0067] Embodiment 11
[0068] The preparation method of a poisoning-resistant organic sulfur hydrogenation catalyst is substantially the same as that of Example 4, except that:
[0069] In step (3), 0.6132 g (NH4)6Mo7O 24 ·4H2O, 1.813g Co(NO3)2·6H2O was dissolved in 50mL of water, 4g of the carrier obtained in step (2) was added, and the finished catalyst was obtained by the same operation as step (3) of Example 4.
[0070] Example 12
[0071] A method for preparing a poisoning-resistant organic sulfur hydrogenation catalyst, which is substantially the same as Example 4, except that:
[0072] (1) The masses of Al(NO3)3·9H2O, Ce(NO3)3·6H2O, and Zr(NO3)4·5H2O were 3.6777 g, 5.0445 g, and 6.9683 g, respectively, and a precipitate was obtained by the same operation as step (1) of Example 4;
[0073] (2) drying the precipitate obtained in step (1) in an oven at 80-100° C. overnight to obtain a powder, and then keeping the powder in a muffle furnace at 550° C. for 4 hours to obtain a carrier;
[0074] (3) 0.6133 g (NH4)6Mo7O 24 ·4H2O, 0.7593g Cu(NO3)2·3H2O and 0.9065g Co(NO3)2·6H2O were dissolved in 50mL of water, 1.3mL Mn(NO3)2 solution was added, and then 3.5g of the carrier obtained in step (2) was added, and the finished catalyst was obtained by the same operation as step (3) of Example 4.
[0075] Comparative Example 1
[0076] A method for preparing a hydrogenation catalyst, the method comprising:
[0077] (1) Dissolve 10 g of Ce(NO3)3·6H2O in 50 mL of water, add 1.3 mL of Mn(NO3)2 solution, add Na2CO3 precipitant to precipitate, add NaOH solution dropwise to adjust the pH value to 10-11, then age at 80°C for 6 h and filter, then wash the precipitate 2-5 times with deionized water to obtain a precipitate;
[0078] (2) Add 0.6132 g (NH4)6Mo7O to the precipitate obtained in step (1) 24 ·4H2O, stir evenly, place the obtained precipitate in an oven at 80-100℃ and dry overnight to obtain powder, then place it in a muffle furnace, heat it to 300℃ at a rate of 2℃ / min and keep it for 1h, then heat it to 550℃ at a rate of 2℃ / min and keep it for 4h to obtain the finished catalyst powder.
[0079] Comparative Example 2
[0080] A method for preparing a hydrogenation catalyst, the method comprising:
[0081] (1) 14.7 g of Al(NO3)3·9H2O and 1.5186 g of Cu(NO3)2·3H2O were dissolved in 50 mL of water, a precipitant was added to precipitate the mixture, a NaOH solution was added dropwise to adjust the pH value to 10-11, the mixture was aged at 80° C. for 6 h, filtered, and then washed 2-5 times with deionized water to obtain a precipitate;
[0082] (2) Add 0.6132 g (NH4)6Mo7O to the precipitate obtained in step (1) 24 ·4H2O, stir evenly, place the obtained precipitate in an oven at 80-100℃ and dry overnight to obtain powder, then place it in a muffle furnace, heat it to 300℃ at a rate of 2℃ / min and keep it for 1h, then heat it to 550℃ at a rate of 2℃ / min and keep it for 4h to obtain the finished catalyst powder.
[0083] Comparative Example 3
[0084] A method for preparing a hydrogenation catalyst, the method comprising:
[0085] (1) 11.1 g Zr(NO3)4·5H2O and 1.813 g Co(NO3)2·6H2O were dissolved in 50 mL of water, and Na2CO3 precipitant was added to precipitate the mixture, and NaOH solution was added dropwise to adjust the pH value to 10-11, and then the mixture was aged at 80°C for 6 h and filtered, and then the precipitate was washed 2-5 times with deionized water to obtain a precipitate;
[0086] (2) Add 0.6132 g (NH4)6Mo7O to the precipitate obtained in step (1) 24·4H2O, stir evenly, place the obtained precipitate in an oven at 80-100℃ and dry overnight to obtain powder, then place it in a muffle furnace, heat it to 300℃ at a rate of 2℃ / min and keep it for 1h, then heat it to 550℃ at a rate of 2℃ / min and keep it for 4h to obtain the finished catalyst powder.
[0087] Experimental Example 1 Characterization of the catalysts prepared with different raw materials and reaction conditions in Examples 1 to 12 and Comparative Examples 1 to 3
[0088] The present invention loads different active components on a carrier to obtain different catalysts. Only the catalysts obtained in Examples 5, 7, 12 and Comparative Example 1 contain MnO2 and MoO3. When the heating rate of calcination in steps (2) and (3) of Examples 1 to 12 and Comparative Examples 1 to 3 is 1 to 5°C / min, the structure of the obtained catalyst is stable. If the temperature is too high, the catalyst will sinter (when the temperature is greater than 700°C, the microstructure of the carrier will change, such as the collapse of the pore structure, the sharp decrease in surface area, or the growth of the grains of the loaded active components, which will eventually lead to aging of the catalyst and gradual loss of activity); if the temperature is lower than 300°C, the precursor salt cannot be completely decomposed into oxides.
[0089] Experimental Example 2 Study on the conditions and results of the catalytic reaction of COS and CS2 by the catalysts prepared in Examples 1 to 12 and Comparative Examples 1 to 3
[0090] 1. Conditions and results of the catalysts of Examples 1 to 12 for catalyzing COS and CS2
[0091] First, the catalysts of Examples 1 to 12 are respectively placed in a reactor, and subjected to a presulfurization treatment in 0.1% to 1% H2S, 99.0 to 99.9% H2, at 350°C for 8 hours to obtain a sulfided catalyst. The sulfidation principle is that the above catalyst is directly contacted with a certain concentration of hydrogen sulfide or other organic sulfide in the presence of hydrogen to perform gas phase sulfidation (since the catalyst is easily oxidized with O2, the transportation and storage of the catalyst are all carried out in the oxidized state. When the catalyst is loaded into the reactor, in order to make the catalyst active, it must be presulfided to change the catalyst from the oxidized state to the sulfided state and restore its activity).
[0092] Then, the activity of the above-mentioned sulfided catalysts was tested at different temperatures. It was only necessary to replace H2S / H2 with the raw gas. The reaction conditions were: the raw gas contained COS, CS2, and H2 / Ar, wherein the volume percentage of COS was 0.02% (the concentration of COS before the reaction was 200ppm), the volume percentage of CS2 was 0.01% (the concentration of CS2 before the reaction was 100ppm), and the volume percentage of H2 in H2 / Ar was 5%; the space velocity was 5000h -1; The reaction temperature is 250-280°C; and it is carried out under normal pressure. The catalytic principle of the catalyst is: COS and CS2 react with H2 to generate H2S and CO2 respectively. The specific calculation formula for the conversion rate of COS and CS2 is as follows:
[0093]
[0094] Among them, C 反应前 are the concentrations of COS and CS2 in the raw gas before the reaction, C 反应后 They are the concentrations of COS and CS2 in the gas after the reaction, both in ppm.
[0095] The specific data of the experimental results are shown in Table 1 (conversion rate of COS) and Table 2 (conversion rate of CS2):
[0096] Table 1 Conditions and results of COS catalyzed by the catalysts of Examples 1 to 12
[0097]
[0098]
[0099] Table 2 Conditions and results of catalytic CS2 of catalysts of Examples 1 to 12
[0100]
[0101] As shown in Tables 1-2, the removal rates of COS and CS2 of the catalysts prepared in Examples 1-12 are between 50% and 70% when the reaction temperature is 250°C; when the reaction temperature is 270°C, the removal rates of COS and CS2 are between 70% and 90%; when the reaction temperature is 280°C, the removal rates of COS and CS2 can reach more than 95%. Comprehensive comparison shows that when the reaction temperature is 250-280°C, the catalysts prepared in Examples 5, 7, and 12 have better effects on catalyzing COS and CS2 than those in other examples. This is because the catalysts prepared in Examples 5, 7, and 12 are all added with Mn and Mo elements, which produce a synergistic effect and improve the activity of the catalyst.
[0102] 2. Conditions and results of catalysis of COS and CS2 by the catalysts prepared in Comparative Examples 1 to 3
[0103] The catalysts prepared in the above comparative examples 1 to 3 were respectively taken to carry out activity tests in the reactor at different temperatures. The remaining reaction conditions and reaction principles were the same as those of the catalysts of the above examples 1 to 12 for catalyzing COS and CS2. The specific data of the experimental results are shown in the following Table 3 (conversion rate of COS) and Table 4 (conversion rate of CS2):
[0104] Table 3 Conditions and results of COS catalyzed by the catalysts of Comparative Examples 1 to 3
[0105]
[0106] Table 4 Conditions and results of catalytic CS2 of the catalysts of Comparative Examples 1 to 3
[0107]
[0108] Table 5 Proportion of each component in the carrier of the catalyst prepared in the examples and comparative examples
[0109]
[0110]
[0111] As shown in Tables 3 to 5, the removal rates of COS and CS2 of the catalysts prepared in Comparative Examples 1 to 3 are between 40% and 50% when the reaction temperature is 250°C; when the reaction temperature is 270°C, the removal rates of COS and CS2 are between 55% and 69%; when the reaction temperature is 280°C, the removal rates of COS and CS2 do not exceed 83%. Comprehensive comparison shows that when the reaction temperature is 250 to 280°C, the catalyst prepared in Comparative Example 1 catalyzes COS and CS2, and the corresponding removal rates are higher than those of Comparative Examples 2 and 3. This is because the catalyst prepared in Comparative Example 1 contains both Mn and Mo elements, and the two produce a synergistic effect, and the catalyst activity is good. However, the effect of the catalyst prepared in Comparative Example 1 on catalyzing COS and CS2 is not as good as that of Examples 5, 7, and 12, because the catalysts in Examples 5, 7, and 12 not only contain MnO2 and MoO3 that produce a synergistic effect, but also the components in the carrier are at least two, while the catalyst prepared in Comparative Example 1 has only one component in the carrier.
[0112] Experimental Example 3 Verifies that the catalyst prepared in Example has long-term effectiveness
[0113] The catalyst prepared in Example 7 of the present invention catalyzes COS, and its 100% conversion rate can be maintained for 50 hours. After 50 hours, the conversion rate slowly decreases, and the conversion rate drops to 80% after 60 hours. The 95% conversion rate of CS2 can be maintained for 55 hours, and the conversion rate slowly decreases after 55 hours, and the conversion rate drops to 80% after 63 hours. Therefore, the catalytic effect of the catalyst prepared in Example 7 of the present invention is not only very good, but also maintained for a long time.
[0114] Experimental Example 3 Verifies that the catalyst prepared in Example has thermal stability
[0115] When the catalyst prepared in Example 7 of the present invention catalyzes COS and CS2, when the catalytic reaction temperature rises to 700° C., the conversion rates of COS and CS2 do not decrease; when the catalytic reaction temperature is greater than 700° C., the conversion rates of COS and CS2 are 100%. Therefore, compared with the hydrolysis method, the catalyst prepared in Example 7 of the present invention has a wider catalytic reaction temperature range and can be applied to higher temperatures, reducing heat loss and achieving the effect of energy saving and emission reduction.
[0116] In summary, the catalyst prepared by the present invention has good thermal stability and long-term effectiveness. When the reaction temperature is above 280° C., the removal rate of COS and CS2 can reach above 95%.
[0117] Although the content of the present invention has been described in detail through the above preferred embodiments, it should be appreciated that the above description should not be considered as a limitation of the present invention. After reading the above content, it will be apparent to those skilled in the art that various modifications and substitutions of the present invention will occur. Therefore, the protection scope of the present invention should be limited by the appended claims.
Claims
1. A poisoning-resistant organic sulfur hydrogenation catalyst, characterized in that: The catalyst comprises: Carrier, active ingredient; Wherein, the carrier is ZrO2, Al2O3 and CeO2 or CeO2 and ZrO2; The active components are MnO2 and MoO3; When the carrier is ZrO2, Al2O3 and CeO2, the mass ratio of ZrO2, Al2O3 and CeO2 is (40-50): (20-30): (20-40); The mass ratio of the carrier to the active component is (45-85): (15-55).
2. The poisoning-resistant organic sulfur hydrogenation catalyst according to claim 1, characterized in that: The mass ratio of the carrier to the active component is 8:
2.
3. The poisoning-resistant organic sulfur hydrogenation catalyst according to claim 1, characterized in that: The active components are MnO2 and MoO3, wherein the mass ratio of MnO2 to MoO3 is (4-15): (5-20).
4. A method for preparing a poisoning-resistant organic sulfur hydrogenation catalyst as claimed in any one of claims 1 to 3, characterized in that: The method includes: (1) dissolving the precursor of the active component and the precursor of the carrier, mixing and adding a precipitant, filtering and washing to obtain a precipitate; or, First, the precursor of the carrier is dissolved, mixed, and a precipitant is added, filtered, and the filter residue is washed, dried, and roasted to obtain a carrier. Then, the precursor of the active component is dissolved, mixed and stirred with the obtained carrier, allowed to stand, and heated and stirred to obtain a precipitate; (2) Drying and calcining the precipitate obtained in step (1) to obtain an anti-poisoning organic sulfur catalyst.
5. The preparation method according to claim 4, characterized in that: The precursors of the active components are soluble salts; the precursors of the carriers are all nitrates.
6. The preparation method according to claim 4, characterized in that: In step (1), the precipitant is sodium carbonate, the drying temperature is 80-100°C, and the calcination temperature is 300-650°C.
7. The preparation method according to claim 4, characterized in that: In step (1), the heating and stirring are performed at 40°C, 50°C, 60°C, and 70°C, respectively, for 1 hour each and with continuous stirring.
8. The preparation method according to claim 4, characterized in that: In step (2), the calcination temperature is 300-700° C. and the calcination time is 4-6 hours.
9. Use of the poisoning-resistant organic sulfur hydrogenation catalyst according to any one of claims 1 to 3 in hydrodesulfurization.