A preparation method and application of dual-ligand hybrid material
The dual ligand hybrid material prepared by one-step method solves the problem of difficult preparation of MOF/MOF hybrid materials in the prior art, and achieves high-efficiency photocatalytic decomposition of water to produce hydrogen, with excellent visible light capture ability and good cycle stability It is suitable for photocatalytic decomposition of water to produce hydrogen.
Patent Information
- Application Number
- CN202211619031.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-16
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-12-16
AI Technical Summary
It is difficult to prepare efficient MOF/MOF hybrid materials by one-step method in the prior art, and their application in the field of photocatalytic decomposition of water hydrogen production has problems with efficiency and stability.
ZrCl4, porphyrin or metalporphyrin, terephthalic acid derivative, benzoic acid and DMF are reacted in a specific molar ratio in a polytetrafluoroethylene reactor, and are prepared by magnetic stirring, heating, cooling, centrifugation and vacuum drying. The biligand hybrid material was discharged and dispersed in TEOA and PBS solutions, and the photocatalytic reaction was performed using a 300 W xenon lamp source.
A one-step preparation of dual ligand hybrid materials was realized, forming a nanorod structure with surface coated nanoparticles, with a large specific surface area and excellent visible light capture capability, and the photocatalytic hydrogen production rate reached 3400μmol g-1 h-1 , good cycle stability and yield is as high as more than 70%.
Smart Images

Figure CN115888838B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of new materials, and specifically relates to a preparation method of a dual-ligand hybrid material and application thereof. Background Art
[0002] Hydrogen is a green and sustainable energy source and is considered to be one of the ideal options for solving the global energy crisis and environmental problems. Solar-driven water splitting to produce hydrogen has attracted widespread attention as a promising mechanism for obtaining hydrogen energy. The key to photocatalytic hydrogen production technology is to develop photocatalysts that can efficiently and stably split water using inexhaustible solar energy. Generally speaking, there are several key processes in the photocatalytic hydrogen production reaction: light absorption by the photocatalyst, generation of photogenerated electron-charge pairs, separation and transfer of photogenerated electron-hole carriers, and reduction of H by active electrons. + Generate H2; therefore, the design of efficient photocatalysts mainly focuses on the improvement of one or more aspects of these key steps. Matching the band structures of different materials to achieve a synergistic effect between them is an effective way to improve the efficiency of photogenerated electron-hole separation.
[0003] MOFs, as a new type of porous crystalline material, has the characteristics of high specific surface area, adjustable pore size and structural diversity. Combining MOFs with other functional materials to obtain MOF-based hybrid materials has become a hot topic of research, especially MOF / MOF hybrid materials. Due to the synergistic effect between different MOFs, they have received widespread attention in the fields of gas adsorption and separation, heterogeneous catalysis, biomedicine and sensing. MOF / MOF, as a new type of MOF-based hybrid material, is currently reported in the literature. Most of the hybrid materials are obtained by step-by-step synthesis methods, which mainly include epitaxial growth methods, kinetic control methods, surfactant-assisted methods and ligand exchange methods. However, there are few reports on the preparation of MOF / MOF hybrid materials by a one-step method. This is because it is difficult to control the size and shape of each MOF component and the selective nucleation and growth of the secondary MOF by the one-step method. Summary of the invention
[0004] In order to overcome the technical defects of the prior art, the present invention proposes a method for preparing a dual-ligand hybrid material, realizes the one-step preparation of the dual-ligand hybrid material, and applies the dual-ligand hybrid material to the field of photocatalytic water decomposition to produce hydrogen.
[0005] To achieve the above object, the technical scheme adopted by the present invention is: a preparation method of a dual-ligand hybrid material, comprising the following steps: adding ZrCl4, porphyrin or metalloporphyrin, terephthalic acid or terephthalic acid derivative, benzoic acid and DMF in a molar ratio of 1:0.25-0.42:0.38-0.76:18.26-42.62:191.34-382.68 to a polytetrafluoroethylene reactor, stirring magnetically for 15-20 min, placing the reactor in a stainless steel reactor, heating the reactor in an oven at 130-140°C for 12-20 h, cooling to room temperature, collecting samples by centrifugation at 5000-7000 rpm / min for 5-10 min, washing the samples with DMF and ethanol for several times, and then drying the samples in a vacuum drying oven at 70-80°C for 48-60 h to obtain the dual-ligand hybrid material;
[0006] Preferably, the terephthalic acid derivatives include (NH2)2-BDC, NH2-BDC, (OH)2-BDC, and the metalloporphyrins include PdTCPP, PtTCPP, CuTCPP, FeTCPP;
[0007] The present invention also provides an application of the dual-ligand hybrid material in photocatalytic hydrogen production, the method comprising: dispersing the dual-ligand hybrid material in a solution composed of TEOA and PBS in a volume ratio of 1:4-7, evacuating the reaction system to a vacuum state with a vacuum pump, and turning on a light source;
[0008] Preferably, the light source is a 300 W xenon lamp with λ≥400 nm.
[0009] The beneficial effects achieved by the present invention are:
[0010] The present invention can realize the one-step preparation of dual-ligand hybrid materials, wherein the dual ligands are MTCPP (M = Pd, Pt, Cu, Fe, 2H) and BDC-N (N = 2NH2, NH2, 2OH, 2H); the morphology of the prepared dual-ligand hybrid material is a nanorod structure with nanoparticles coated on the surface, and the size is uniform and can be controlled at 6~10μm; the formation process of the hybrid material is: first, PCN-222(M) nanorods are formed, and then the unsaturated Zr6 clusters on the surface of PCN-222(M) react with COOH at one end of BDC-N, and COOH at the other end of BDC-N forms new Zr6 clusters in the presence of Zr source, and the newly formed Zr6 clusters continue to react with BDC-N to finally form UiO-66-N, and the result is that some UiO-66-N connected by chemical bonds are formed on the surface of PCN-222(M) (the internal steric hindrance of the skeleton is large and the possibility is small); the dual-ligand hybrid material has a large specific surface area and excellent visible light capture ability, and is suitable for photocatalytic water decomposition to produce hydrogen. Under visible light irradiation, the photocatalytic hydrogen production rate reaches up to 3400μmol g -1 h -1 The cycle stability performance test found that the hydrogen production rate did not decrease significantly after four cycles, and had good cycle stability; the preparation process of the present invention is simple and feasible, with a yield of more than 70%, and is worthy of market promotion. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] Figure 1 TEM image of the hybrid material (NH2)2-UiO-66 / PCN-222(Pd) of Example 1 of the present invention;
[0012] Figure 2 This is the UV-visible absorption spectrum of the hybrid material (NH2)2-UiO-66 / PCN-222(Pd) of Example 1 of the present invention;
[0013] Figure 3 This is a graph showing the rate of photocatalytic water decomposition and hydrogen production by the hybrid material (NH2)2-UiO-66 / PCN-222 (Pd) of Example 1 of the present invention;
[0014] Figure 4 This is a comparison chart of the four cycle activities of the hybrid material (NH2)2-UiO-66 / PCN-222 (Pd) for photocatalytic water decomposition to produce hydrogen in Example 1 of the present invention;
[0015] Figure 5 TEM image of the hybrid material (NH2)2-UiO-66 / PCN-222(Pt) of Example 2 of the present invention;
[0016] Figure 6TEM image of the hybrid material (NH2)2-UiO-66 / PCN-222(Cu) of Example 3 of the present invention;
[0017] Figure 7 TEM image of the hybrid material (NH2)2-UiO-66 / PCN-222(Fe) of Example 4 of the present invention;
[0018] Figure 8 TEM image of the hybrid material (NH2)2-UiO-66 / PCN-222 of Example 5 of the present invention;
[0019] Fig. 9 TEM image of the hybrid material NH2-UiO-66 / PCN-222 (Pd) of Example 6 of the present invention;
[0020] Fig.10 TEM image of the hybrid material (OH)2-UiO-66 / PCN-222(Pd) of Example 7 of the present invention;
[0021] Fig.11 TEM image of the hybrid material NH2-UiO-66 / PCN-222(Fe) of Example 8 of the present invention;
[0022] Fig.12 TEM image of the hybrid material UiO-66 / PCN-222 (Fe) of Example 9 of the present invention;
[0023] Fig.13 XRD spectra of 9 hybrid materials in the embodiments of the present invention;
[0024] Fig.14 is the SEM image of Example 10 of the present invention;
[0025] Fig.15 This is the SEM image of Example 11 of the present invention;
[0026] Fig.16 This is the SEM image of Example 12 of the present invention;
[0027] Fig.17 This is the SEM image of Example 13 of the present invention. DETAILED DESCRIPTION
[0028] The present invention will be further described below by means of specific examples.
[0029] Example 1: Preparation of hybrid material (NH2)2-UiO-66 / PCN-222(Pd)
[0030] ZrCl4 (30 mg), PdTCPP (30 mg), (NH2)2-BDC (10 mg), benzoic acid (700 mg) and DMF (2 mL) were added to a 20 mL polytetrafluoroethylene reactor and stirred for 15 min. Then the reactor was transferred to a reactor, which was heated in an oven at 130 °C for 12 h. After the temperature was cooled to room temperature, the product was collected by centrifugation. The product was washed three times with DMF and ethanol respectively. Finally, the product was placed in a vacuum drying oven at 70 °C for 48 h. The product was the hybrid material (NH2)2-UiO-66 / PCN-222(Pd); the yield was 73%.
[0031] Example 2: Preparation of hybrid material (NH2)2-UiO-66 / PCN-222(Pt)
[0032] ZrCl4 (30 mg), PtTCPP (30 mg), (NH2)2-BDC (10 mg), benzoic acid (700 mg) and DMF (2 mL) were added to a 20 mL polytetrafluoroethylene reactor and stirred for 15 min. Then the reactor was transferred to an autoclave, which was heated in an oven at 130 °C for 12 h. After the temperature was cooled to room temperature, the product was collected by centrifugation. The product was washed three times with DMF and ethanol respectively. Finally, the product was placed in a vacuum drying oven at 70 °C for 48 h. The product was the hybrid material (NH2)2-UiO-66 / PCN-222(Pt); the yield was 76%.
[0033] Example 3: Preparation of hybrid material (NH2)2-UiO-66 / PCN-222(Cu)
[0034] ZrCl4 (30 mg), CuTCPP (30 mg), (NH2)2-BDC (10 mg), benzoic acid (700 mg) and DMF (2 mL) were added to a 20 mL polytetrafluoroethylene reactor and stirred for 15 min. Then the reactor was transferred to a reactor, which was heated in an oven at 130 °C for 12 h. After the temperature was cooled to room temperature, the product was collected by centrifugation. The product was washed three times with DMF and ethanol respectively. Finally, the product was placed in a vacuum drying oven at 70 °C for 48 h. The product was the hybrid material (NH2)2-UiO-66 / PCN-222(Cu); the yield was 71%.
[0035] Example 4: Preparation of hybrid material (NH2)2-UiO-66 / PCN-222(Fe)
[0036] ZrCl4 (30 mg), FeTCPP (30 mg), (NH2)2-BDC (10 mg), benzoic acid (700 mg) and DMF (2 mL) were added to a 20 mL polytetrafluoroethylene reactor and stirred for 15 min. The reactor was then transferred to a reactor and heated in an oven at 130 °C for 12 h. After the temperature was cooled to room temperature, the product was collected by centrifugation. The product was washed three times with DMF and ethanol respectively. Finally, the product was placed in a vacuum drying oven at 70 °C for 48 h, and the obtained product was the hybrid material (NH2)2-UiO-66 / PCN-222(Fe); the yield was 75%.
[0037] Example 5: Preparation of hybrid material (NH2)2-UiO-66 / PCN-222
[0038] ZrCl4 (30 mg), TCPP (30 mg), (NH2)2-BDC (10 mg), benzoic acid (700 mg) and DMF (2 mL) were added to a 20 mL polytetrafluoroethylene reactor and stirred for 15 min. The reactor was then transferred to a reactor. The reactor was heated in an oven at 130 °C for 12 h. After the temperature was cooled to room temperature, the product was collected by centrifugation and washed three times with DMF and ethanol respectively. Finally, the product was placed in a vacuum drying oven at 70 °C for 48 h. The product obtained was the hybrid material (NH2)2-UiO-66 / PCN-222; the yield was 79%.
[0039] Example 6: Preparation of hybrid material NH2-UiO-66 / PCN-222 (Pd)
[0040] ZrCl4 (30 mg), PdTCPP (30 mg), NH2-BDC (10 mg), benzoic acid (300 mg) and DMF (2 mL) were added to a 20 mL polytetrafluoroethylene reactor and stirred for 15 min. Then the reactor was transferred to a reactor, and the reactor was heated in an oven at 130 °C for 12 h. After the temperature was cooled to room temperature, the product was collected by centrifugation. The product was washed three times with DMF and ethanol respectively. Finally, the product was placed in a vacuum drying oven at 70 °C for 48 h. The product was the hybrid material NH2-UiO-66 / PCN-222 (Pd); the yield was 75%.
[0041] Example 7: Preparation of hybrid material (OH)2-UiO-66 / PCN-222(Pd)
[0042] ZrCl4 (30 mg), PdTCPP (30 mg), (OH)2-BDC (10 mg), benzoic acid (700 mg) and DMF (2 mL) were added to a 20 mL polytetrafluoroethylene reactor and stirred for 15 min. Then the reactor was transferred to a reactor, which was heated in an oven at 130 °C for 12 h. After cooling to room temperature, the product was collected by centrifugation. The product was washed three times with DMF and ethanol respectively. Finally, the product was placed in a vacuum drying oven at 70 °C for 48 h. The product was the hybrid material (OH)2-UiO-66 / PCN-222(Pd); the yield was 81%.
[0043] Example 8: Preparation of NH2-UiO-66 / PCN-222(Fe) hybrid material
[0044] ZrCl4 (30 mg), FeTCPP (30 mg), NH2-BDC (10 mg), benzoic acid (300 mg) and DMF (2 mL) were added to a 20 mL polytetrafluoroethylene reactor and stirred for 15 min. Then the reactor was transferred to a reactor, which was heated in an oven at 130 °C for 12 h. After the temperature was cooled to room temperature, the product was collected by centrifugation. The product was washed three times with DMF and ethanol respectively. Finally, the product was placed in a vacuum drying oven at 70 °C for 48 h. The product was the hybrid material NH2-UiO-66 / PCN-222(Fe); the yield was 72%.
[0045] Example 9: Preparation of hybrid material UiO-66 / PCN-222(Fe)
[0046] ZrCl4 (30 mg), FeTCPP (30 mg), BDC (10 mg), benzoic acid (300 mg) and DMF (2 mL) were added to a 20 mL polytetrafluoroethylene reactor and stirred for 15 min. The reactor was then transferred to an autoclave, which was heated in an oven at 130 °C for 12 h. After cooling to room temperature, the product was collected by centrifugation and washed three times with DMF and ethanol respectively. Finally, the product was placed in a vacuum drying oven at 70 °C for 48 h. The product was the hybrid material UiO-66 / PCN-222(Fe); the yield was 77%.
[0047] Example 10: The raw materials commonly used in the industry for preparing (NH2)2-UiO-66 separately were mixed according to the commonly used ratio and the raw materials commonly used in the industry for preparing PCN-222 (Pd) separately were mixed according to the commonly used ratio, and the experiment was carried out according to the reaction conditions of Example 1;
[0048] ZrCl4 (80 mg), PdTCPP (50 mg), (NH2)2-BDC (10 mg), benzoic acid (700 mg) and DMF (2 mL) were added to a 20 mL polytetrafluoroethylene reactor and stirred for 15 min. The reactor was then transferred to a reactor. The reactor was heated in an oven at 130 °C for 12 h. After the temperature was cooled to room temperature, the product was collected by centrifugation. The product was washed three times with DMF and ethanol respectively. Finally, the product was placed in a vacuum drying oven at 70 °C for 48 h. Fig.14 It can be seen that the experimental results are quite different from those in Example 1, no hybrid material is formed, and (NH2)2-UiO-66 and PCN-222(Pd) exist independently.
[0049] Example 11: Based on Example 1, the raw materials required for the synthesis of PCN-222 (Pd) were deleted and replaced with "synthesized PCN-222 (Pd)", and the experiment was carried out according to the reaction conditions of Example 1;
[0050] PCN-222(Pd) (20 mg), ZrCl4 (10 mg), (NH2)2-BDC (10 mg), benzoic acid (700 mg) and DMF (2 mL) were added to a 20 mL polytetrafluoroethylene reactor and stirred for 15 min. The reactor was then transferred to a reactor. The reactor was heated in an oven at 130 °C for 12 h. After the temperature was cooled to room temperature, the product was collected by centrifugation. The product was washed three times with DMF and ethanol respectively. Finally, the product was placed in a vacuum drying oven at 70 °C for 48 h. Fig.15 It can be seen that the experimental results are quite different from those in Example 1, and PCN-222(Pd) shows that only a small amount of (NH2)2-UiO-66 is formed.
[0051] Example 12: The prepared (NH2)2-UiO-66 and PCN-222(Pd) were directly mixed and the experiment was carried out according to the reaction conditions of Example 1;
[0052] PCN-222(Pd) (30 mg), (NH2)2-UiO-66 (20 mg), benzoic acid (700 mg) and DMF (2 mL) were added to a 20 mL polytetrafluoroethylene reactor and stirred for 15 min. The reactor was then transferred to a reactor. The reactor was heated in an oven at 130 °C for 12 h. After the temperature was cooled to room temperature, the product was collected by centrifugation. The product was washed three times with DMF and ethanol respectively. Finally, the product was placed in a vacuum drying oven at 70 °C for 48 h. Fig.16It can be seen that the experimental results are quite different from those in Example 1, no hybrid material is formed, and (NH2)2-UiO-66 and PCN-222(Pd) exist independently.
[0053] Example 13: Based on Example 1, (NH2)2-BDC is added in excess;
[0054] ZrCl4 (30 mg), PdTCPP (30 mg), (NH2)2-BDC (50 mg), benzoic acid (700 mg) and DMF (2 mL) were added to a 20 mL polytetrafluoroethylene reactor and stirred for 15 min. The reactor was then transferred to a reactor. The reactor was heated in an oven at 130 °C for 12 h. After the temperature was cooled to room temperature, the product was collected by centrifugation. The product was washed three times with DMF and ethanol respectively. Finally, the product was placed in a vacuum drying oven at 70 °C for 48 h. Fig.17 It can be seen that compared with Example 1, in addition to the formation of hybrid materials, a large amount of free (NH2)2-UiO-66 will appear due to the addition of a large amount of (NH2)2-BDC.
[0055] 5 mg of (NH2)2-UiO-66 / PCN-222(Pd) prepared in Example 1 was dispersed in a mixed solution of 20 mL TEOA and 80 mL PBS and ultrasonically dispersed. The reaction system was evacuated to vacuum with a vacuum pump, and the light source (300 W xenon lamp, λ ≥ 400 nm) was turned on. The reaction temperature was maintained at about 6 °C by a constant temperature cooling circulation pump, and the hydrogen content during the reaction was measured by online gas chromatography (GC-7920, TCD). The results showed that (NH2)2-UiO-66 / PCN-222(Pd) exhibited excellent photocatalytic hydrogen production performance, and its hydrogen production rate was as high as 3400 μmol g -1 h -1 The reason why the hybrid material has high photocatalytic performance is attributed to the hybrid material composed of PCN-222(Pd) and UiO-66-(NH2)2. UiO-66-(NH2)2 can act as a photosensitizer, and more photogenerated electrons are involved in the hydrogen production reaction by decomposing water.
[0056] The above specific implementation modes are used to explain the present invention rather than to limit the present invention. Any modification and change made to the present invention within the spirit of the present invention and the protection scope of the claims shall fall within the protection scope of the present invention.
Claims
1. A method for preparing a dual-ligand hybrid material, It is characterized in that The following steps are involved: ZrCl 4 , porphyrin or metalloporphyrin, terephthalic acid or terephthalic acid derivative, benzoic acid and DMF are added into a polytetrafluoroethylene reactor in a molar ratio of 1:0.25-0.42:0.38-0.76:18.26-42.62:191.34-382.
68. The terephthalic acid derivative includes (NH 2 ) 2 -BDC, NH 2 -BDC, (OH) 2 -BDC, magnetically stir for 15-20 min, then place the reactor in a stainless steel reactor, heat the reactor in an oven at 130-140°C for 12-20 h, cool to room temperature, collect the sample by centrifugation at 5000-7000 rpm for 5-10 min, wash the sample with DMF and ethanol several times, and then dry the sample in a vacuum drying oven at 70-80°C for 48-60 h to obtain the dual ligand hybrid material.
2. The preparation method according to claim 1, It is characterized in that The metal porphyrins include PdTCPP, PtTCPP, CuTCPP and FeTCPP.
3. A dual-ligand hybrid material prepared by the preparation method described in any one of claims 1-2.
4. Use of the dual-ligand hybrid material according to claim 3 in photocatalytic hydrogen production.
5. The use according to claim 4, It is characterized in that The method is as follows: the dual-ligand hybrid material is added into a solution composed of TEOA and PBS in a volume ratio of 1:4-7, the reaction system is evacuated to a vacuum state using a vacuum pump, and then the light source is turned on.
6. The use according to claim 5, It is characterized in that The light source is a 300 W xenon lamp with λ≥400 nm.