A polyurea composition and its preparation method and application
By introducing nanotitanium dioxide hybrid polyaluminum titanium siloxane and inorganic pigments into polyurea materials, combined with fluorosilane coupling agent, the water repellent, water repellent and temperature resistance of polyurea materials are improved, and the existing poly 脲材料的性能不足问题,实现了更好的防腐性能和物理性能。
Patent Information
- Application Number
- CN202211476722.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-23
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-11-23
AI Technical Summary
The existing polyurea materials have water repellent, insufficient water repellent capacity, average temperature resistance, low flame retardant grade, need to be improved, and are insensitive to moisture and temperature.
The isocyanate component is combined with nanotitanium dioxide hybrid polyaluminum titanium siloxane and inorganic pigment to prepare inorganic pigments through reaction of fluorosilane coupling agent, which significantly improves the water repellent and water repellent ability of the material, and is in the polyurea macromolecular structure. Si-O-Al-O-Ti-O segments are introduced to form a highly viscous liquid or paste-like material.
It significantly improves the temperature resistance, flame retardant and flexibility of polyurea materials, and has the characteristics of rapid curing, moisture and temperature insensitive, and improves corrosion resistance and physical properties.
Smart Images

Figure QLYQS_1 
Figure QLYQS_2 
Figure QLYQS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of anti-corrosion materials, and in particular to a polyurea composition and a preparation method and application thereof. Background Art
[0002] Polyurea elastomer technology was developed on the basis of reaction injection molding in the mid-to-late 1980s. The American Polyurea Development Association defines polyurea elastomer as follows: polyurea elastomer is an elastomer material generated by the reaction of isocyanate components and amino compound components. The isocyanate component can be a monomer, an isocyanate derivative, or a prepolymer. The elastomer material has excellent physical and chemical properties, such as mechanical properties, wear resistance, corrosion resistance, etc. It does not contain a catalyst and is not affected by ambient temperature and humidity during construction. However, the existing polyurea materials also have some shortcomings, such as low crosslinking density, general chemical structure stability, and low wetting ability for the substrate. In order to break through the single limitation of the material, improve the comprehensive performance and expand the scope of application, it is necessary to use other materials for modification. At present, the materials used to modify polyurea are mainly acrylic acid, epoxy resin, etc. Although certain results have been achieved and the performance of the modified polyurea elastomer materials has been improved to a certain extent, the existing modified polyurea elastomer materials have insufficient water repellency and water repellency, general temperature resistance, can only be used below 150°C, and have a low flame retardant grade and mechanical strength that needs to be improved. Summary of the invention
[0003] The object of the present invention is to overcome one or more deficiencies in the prior art and to provide an improved polyurea composition.
[0004] The present invention also provides a method for preparing the polyurea composition.
[0005] The present invention also provides an application of the polyurea composition in anti-corrosion materials, for example, for the anti-corrosion of various metal chemical equipment in the petroleum and chemical industries, such as storage tanks, pickling tanks, crude oil tanks, gas pipelines, coastal steel structures, offshore drilling platforms, etc. in petroleum, chemical, and steel enterprises.
[0006] In order to achieve the above object, a technical solution adopted by the present invention is:
[0007] A polyurea composition comprises an isocyanate component and an amino compound component, wherein the isocyanate component comprises a prepolymer and an inorganic pigment, and the raw materials of the prepolymer include: polyisocyanate, polyol, and nano-titanium dioxide hybrid polyaluminum titanium siloxane represented by formula (I);
[0008]
[0009] Wherein, X1, X2, X3, X4, and X5 are independently selected from the following groups:
[0010] There are terminal hydroxyl groups in X1, X2, X3, X4, and X5, and any two of them are not repeated, and at least one of the;
[0011] t1, t2, t3, t4, t5 are independently selected from 0-100, and are not 0 when the corresponding group contains aluminum or titanium;
[0012] R1, R2, R3, R4, R5, R6, R7, R8, and R9 are independently selected from C 1-20 Alkyl, phenyl, C 1-6 Alkyl substituted phenyl, C 2-10 alkenyl;
[0013] M is titanium dioxide, which is connected to silicon hydroxyl group, aluminum hydroxyl group or titanium hydroxyl group through hydrogen bonds via hydroxyl groups on the surface.
[0014] In the present invention, the presence of terminal hydroxyl groups in X1, X2, X3, X4, and X5 may refer to the presence of silanol, aluminum hydroxyl, titanium hydroxyl, etc. in the segment structure, or may refer to the hydroxyl groups on the surface of nano-titanium dioxide.
[0015] In some embodiments of the invention, t1, t2, t3, t4, and t5 are independently selected from 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, and 20.
[0016] According to some preferred aspects of the present invention, in formula (I), t1, t2, t3, t4 and t5 are independently selected from 0-50, further 0-30, and further 0-20.
[0017] According to some preferred aspects of the present invention, in formula (I), R1, R2, R3, R4, R5, R6, R7, R8, and R9 are independently selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, n-pentyl, isopentyl, neopentyl, n-hexyl, phenyl, C 1-6 Alkyl-substituted phenyl, vinyl, methyl vinyl, ethyl vinyl, propyl vinyl.
[0018] According to some preferred aspects of the present invention, the average molecular weight of the nano-titanium dioxide hybrid polyaluminum titanium siloxane represented by formula (I) is 500-10000, further 800-8000, and further 1000-5000.
[0019] In some embodiments of the present invention, the average molecular weight of the nano-titanium dioxide hybrid polyaluminum titanium siloxane represented by formula (I) is 1500-4500.
[0020] According to the present invention, the nano-titanium dioxide hybrid polyaluminum titanium siloxane represented by formula (I) of the present invention can be in the form of a highly viscous liquid or paste.
[0021] According to some preferred aspects of the present invention, the mass ratio of the polyol to the nano-titanium dioxide hybrid polyaluminum titanium siloxane represented by formula (I) is 2-10:1.
[0022] According to some preferred aspects of the present invention, the mass percentage of isocyanate groups in the prepolymer is 5%-20%.
[0023] According to some preferred aspects of the present invention, the inorganic pigment is made by reacting a pigment matrix with a fluorosilane coupling agent. This method can significantly improve the hydrophobicity and water repellency of the material. Practice has shown that the contact angle between the material and water can be made greater than 100°, so that the polyurea material has hydrophobicity and water repellency, breaking through the limitations of the use of existing polyurea materials.
[0024] Furthermore, the fluorosilane coupling agent includes at least one of perfluorooctyltriethoxysilane, tridecafluorooctyltriethoxysilane, and perfluorodecyltriethoxysilane.
[0025] In some embodiments of the present invention, the method for preparing the inorganic pigment comprises: adding a pigment matrix dried under vacuum, a fluorosilane coupling agent accounting for about 5-15% of the mass fraction of the pigment matrix, and reflux xylene 10-30 times the amount of the pigment matrix to a three-necked flask equipped with a stirring paddle and a reflux condenser. Raise the temperature to 80-90°C, drip the catalyst trifluoroacetic acid in the formula within 10-60 minutes, and raise the temperature to 110-120°C for reflux reaction. Then filter out the pigment matrix, remove the solvent and excess ungrafted fluorosilane coupling agent, dry in a vacuum oven, and seal for reuse to obtain the inorganic pigment.
[0026] In some embodiments of the present invention, the pigment matrix may be cadmium red pigment or the like.
[0027] According to some preferred aspects of the present invention, the amino compound component comprises an amino-terminated polyether and an optional amine chain extender.
[0028] Further, the amino compound component comprises polyoxypropylene diamine and selectively comprises at least one of 3,5-diethyl-2,4-diaminotoluene, 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, 4,4'-diaminodicyclohexylmethane and 4,4'-bis-sec-butylaminodiphenylmethane.
[0029] According to some preferred aspects of the present invention, the mass ratio of the isocyanate component to the amino compound component is 1:0.5-2.
[0030] Another technical solution provided by the present invention is a method for preparing the polyurea composition described above, which includes a preparation process of an isocyanate component, and the preparation process of the isocyanate component includes: mixing and reacting polyisocyanate, polyol, and nano-titanium dioxide hybrid polyaluminum titanium siloxane represented by formula (I) to generate a prepolymer, and then mixing with an inorganic pigment.
[0031] According to some preferred aspects of the present invention, the preparation method of the nano-titanium dioxide hybrid polyaluminum titanium siloxane represented by formula (I) comprises: subjecting the alkoxysilane to alcoholysis reaction and pre-condensation reaction in water, and then performing the following steps:
[0032] Add (R 1 O)3Al and (R 2 O)4Ti, react, and then add (R 1 O)3Al and (R 2 O) another one of 4Ti, reacting to form the nano titanium dioxide hybrid polyaluminum titanium siloxane represented by the formula (I);
[0033] or,
[0034] Add (R 1 O)3Al and (R 2 O)4Ti, reacting to form the nano titanium dioxide hybrid polyaluminum titanium siloxane represented by the formula (I);
[0035] R 1 Selected from C 3-6 Alkyl, R 2 Selected from C 3-6 alkyl.
[0036] According to some preferred aspects of the present invention, the alkoxysilane may include dialkyltrialkylsilane and optionally alkenyltrialkylsilane and / or aromatictrialkylsilane; in some embodiments, the alkoxysilane may also include dialkenyltetraalkyldisiloxane and / or hexaalkyldisiloxane.
[0037] Furthermore, the alkoxysilane comprises:
[0038] (1) diphenyldimethoxysilane and / or dimethyldimethoxysilane;
[0039] (2) optionally including vinyltrimethoxysilane and / or phenyltrimethoxysilane;
[0040] (3) At least one of divinyltetramethyldisiloxane, hexaphenyldisiloxane and hexamethyldisiloxane.
[0041] In the present invention, the hydrocarbon group includes alkyl, alkenyl, alkynyl, aromatic group and the like. The alkyl group can be methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, n-pentyl, neopentyl, isopentyl, n-hexyl, isohexyl and the like. The alkenyl group can be vinyl, methyl vinyl, ethyl vinyl, propyl vinyl, isopropyl vinyl and the like. The aromatic group includes phenyl and the like.
[0042] According to some preferred and specific aspects of the present invention, R 1 is n-propyl, isopropyl, n-butyl or isobutyl, R 2 It is n-propyl, n-butyl or n-pentyl.
[0043] In some embodiments of the present invention, (R 1 O)3Al can be aluminum isopropoxide.
[0044] In some embodiments of the present invention, (R 2 O)4Ti can be n-butyl titanate.
[0045] According to some preferred aspects of the present invention, the alcoholysis reaction or the pre-condensation reaction is controlled to be carried out at a temperature of 80-95°C.
[0046] According to some preferred aspects of the present invention, adding (R 1 O)3Al or (R 2 After O)4Ti, the temperature of each reaction was controlled at 75-85°C.
[0047] According to some preferred aspects of the present invention, the (R 1 O)3Al and the (R 2 The molar ratio of (R 1 O)3Al and the (R 2 The feeding molar ratio of O)4Ti is 1:0.5-2.
[0048] According to some preferred aspects of the present invention, the molar ratio of silicon to aluminum in the nano-titanium dioxide hybrid polyaluminum titanium siloxane of formula (I) is controlled to be 3-10: 1. Further, the molar ratio of silicon to aluminum in the nano-titanium dioxide hybrid polyaluminum titanium siloxane of formula (I) is controlled to be 4-9: 1.
[0049] In some preferred embodiments of the present invention, the preparation method comprises: adding water and a hydrolysis catalyst into a reactor, heating to a preset reaction temperature, adding alkoxysilane dropwise, refluxing the reaction and removing the generated alcohol substances, and then adding (R 1O)3Al, continue the reflux reaction and remove the generated alcohols, then add (R 2 O)4Ti, continue the reflux reaction and remove the generated alcohol substances, cool to room temperature after the reaction is completed, use organic solvent extraction to remove the water layer, and separate the nano titanium dioxide hybrid polyaluminum titanium siloxane shown in formula (I) from the organic layer.
[0050] In some embodiments of the present invention, the hydrolysis catalyst may be glacial acetic acid or trifluoroacetic acid.
[0051] In some embodiments of the present invention, the water may be distilled water.
[0052] In some embodiments of the present invention, the alkoxysilane is added dropwise within 15-30 minutes.
[0053] In some embodiments of the present invention, the organic solvent is xylene and / or acetylacetone.
[0054] In some embodiments of the present invention, the method for separating the nano-titanium dioxide hybrid polyaluminum titanium siloxane represented by formula (I) from the organic layer can be vacuum distillation to remove xylene or acetylacetone and low molecular weight substances.
[0055] In some embodiments of the present invention, the polyurea composition comprises an isocyanate component and an amino compound component, and the mass ratio of the isocyanate component to the amino compound component is 1:0.5-2;
[0056] The raw materials of the isocyanate component include, by weight: 150-350 parts of polyisocyanate, 120-200 parts of polyol, 10-80 parts of nano-titanium dioxide hybrid polyaluminum titanium siloxane represented by formula (I), and 10-50 parts of inorganic pigment;
[0057] Calculated by weight, the raw materials of the amino compound component include: 70-120 parts of terminal amino polyether and 0-15 parts of amine chain extender.
[0058] Furthermore, the polyurea composition comprises an isocyanate component and an amino compound component, and the mass ratio of the isocyanate component to the amino compound component is 1:0.8-1.5;
[0059] The raw materials of the isocyanate component include, by weight: 180-320 parts of polyisocyanate, 130-185 parts of polyol, 15-70 parts of nano-titanium dioxide hybrid polyaluminum titanium siloxane represented by formula (I), and 15-45 parts of inorganic pigment;
[0060] Calculated by weight, the raw materials of the amino compound component include: 80-105 parts of terminal amino polyether and 3-12 parts of amine chain extender.
[0061] In some embodiments of the present invention, the polyisocyanate may be a diisocyanate, for example, toluene diisocyanate (TDI), isophorone diisocyanate (IPDI), diphenylmethane diisocyanate (MDI), dicyclohexylmethane diisocyanate (HMDI), hexamethylene diisocyanate (HDI), lysine diisocyanate (LDI), etc. In some embodiments of the present invention, the polyol is a hydroxyl-terminated polyether polyol, and may further be a combination of a diol and a triol.
[0062] According to a specific aspect of the present invention, the polyol is composed of polypropylene oxide ether diol and polypropylene oxide ether triol, and the feed mass ratio of the polypropylene oxide ether diol to the polypropylene oxide ether triol is 1.1-2.8:1.
[0063] Another technical solution provided by the present invention is an application of the polyurea composition described above in anti-corrosion materials.
[0064] Due to the application of the above technical solution, the present invention has the following advantages compared with the prior art:
[0065] In view of the shortcomings of existing modified polyurea materials, the present invention adopts in-situ hybrid polymerization technology to introduce Si-O-Al-O-Ti-O chain segments and nano-titanium dioxide hybrid structures into the polyurea macromolecular structure. Practice has found that the polyurea material obtained in this way not only has greatly improved heat resistance and flame retardancy, but also has greatly improved flexibility; it also has the characteristics of fast curing speed, insensitivity to moisture and temperature, good thermal stability, excellent anti-corrosion performance and good physical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0066] Figure 1 The nano titanium dioxide hybrid polyaluminium titanium siloxane prepared in Example 1 1 H-NMR spectrum. DETAILED DESCRIPTION
[0067] The above scheme is further described below in conjunction with specific embodiments; it should be understood that these embodiments are used to illustrate the basic principles, main features and advantages of the present invention, and the present invention is not limited to the scope of the following embodiments; the implementation conditions adopted in the embodiments can be further adjusted according to specific requirements, and the implementation conditions not specified are usually the conditions in conventional experiments.
[0068] Unless otherwise specified in the following examples, all raw materials are commercially available or prepared by conventional methods in the art.
[0069] In the following, diphenyldimethoxysilane was purchased from Aite (Shandong) New Materials Co., Ltd.; dimethyldimethoxysilane was purchased from Hangzhou Guibao Chemical Co., Ltd.; vinyltrimethoxysilane was purchased from Nanjing Ron Silicon Materials Co., Ltd.; phenyltrimethoxysilane was purchased from Zhejiang Woxingman New Materials Technology Co., Ltd.; divinyltetramethyldisiloxane was purchased from Hangzhou Guibao New Materials Co., Ltd.; hexamethyldisiloxane was purchased from Hangzhou Guibao New Materials Co., Ltd.; aluminum isopropoxide was purchased from Yangzhou Zhongtianli New Materials Co., Ltd.; and n-butyl titanate was purchased from Shandong Xinyingshun New Materials Co., Ltd.
[0070] Example 1
[0071] This embodiment provides a nano-titanium dioxide hybrid polyaluminium titanium siloxane and a preparation method thereof. The raw material formula of the nano-titanium dioxide hybrid polyaluminium titanium siloxane is shown in Table 1.
[0072] Table 1
[0073]
[0074]
[0075] The reaction schematic process of the nano-titanium dioxide hybrid polyaluminum titanium siloxane is as follows:
[0076]
[0077] In the above-illustrated reaction process, only the way in which aluminum hydroxyl groups and silicon hydroxyl groups are respectively hydrogen-bonded to titanium dioxide particles through hydroxyl groups on the surface of titanium dioxide is given as an example. In the actual reaction process, Ti-OH on the main chain can also be hydrogen-bonded to titanium dioxide particles through hydroxyl groups on the surface of titanium dioxide. The feed amount is controlled so that there are unconnected terminal hydroxyl groups in the structure, which is the same as the following embodiments.
[0078] The preparation method specifically comprises:
[0079] The formulated amount of distilled water and hydrolysis catalyst (acetic acid) were added to a 1000 mL three-necked flask, heated to 85° C., and a mixed solution of all alkoxysilanes in Table 1 was added dropwise using a dropping funnel, and the dripping was completed in about 25 min. The mixture was stirred and refluxed at 80° C. to remove the alcohol generated by the reaction, and the reaction was continued for 2 h. Subsequently, the formulated amount of aluminum isopropoxide was added to the flask, and the reflux and alcohol-producing reaction was continued for 2 h. Then, the formulated amount of n-butyl titanate was added, and the reflux and alcohol-producing reaction was continued for 2 h. The reaction was completed. After the product was cooled to room temperature, it was extracted with excess xylene to remove the water layer. Finally, the organic layer was distilled under reduced pressure in a rotary evaporator to remove xylene and low molecular weight substances to obtain nano-titanium dioxide hybrid polyaluminum titanium siloxane, 154.29 g, with a yield of 90.02% (theoretical yield is 171.39 g). 1H-NMR spectrum Figure 1 As shown, the average molecular weight measured by GPC (gel permeation chromatography) is 1839, and it is a viscous liquid at 25°C.
[0080] Example 2
[0081] This embodiment provides a nano-titanium dioxide hybrid polyaluminium titanium siloxane and a preparation method thereof. The raw material formula of the nano-titanium dioxide hybrid polyaluminium titanium siloxane is shown in Table 2.
[0082] Table 2
[0083] Raw material name Feeding amount (g) Phenyltrimethoxysilane 110.67 Dimethyldimethoxysilane 19.93 Diphenyldimethoxysilane 32.79 Aluminum Isopropylate 28.98 Distilled water 48.6 n-Butyl Titanate 48.31 Divinyltetramethyldisiloxane 7.69 Acetylacetone 355.31 Trifluoroacetic acid 0.6523
[0084] The reaction schematic process of the nano-titanium dioxide hybrid polyaluminum titanium siloxane is as follows:
[0085]
[0086] The preparation method specifically comprises:
[0087] The formulated amount of distilled water and a hydrolysis catalyst (trifluoroacetic acid) were added to a 1000 mL three-necked flask, heated to 85° C., and a mixed solution of all alkoxysilanes in Table 2 was added dropwise using a dropping funnel, and the dripping was completed in about 25 min. The mixture was stirred and refluxed at 80° C. to remove the alcohol generated by the reaction, and the reaction was continued for 2 h. Subsequently, the formulated amount of aluminum isopropoxide was added to the flask, and the reflux and alcohol-producing reaction was continued for 2 h. Then, the formulated amount of n-butyl titanate was added, and the reflux and alcohol-producing reaction was continued for 2 h. The reaction was completed. After the product was cooled to room temperature, it was extracted with excess acetylacetone to remove the water layer. Finally, the organic layer was distilled under reduced pressure in a rotary evaporator to remove acetylacetone and low molecular weight substances to obtain nano-titanium dioxide hybrid polyaluminum titanium siloxane, 135.28 g, with a yield of 89.79% (theoretical yield of 150.67 g), and the average molecular weight measured by GPC (gel permeation chromatography) was 3568, and it was a paste at 25° C.
[0088] Comparative Example 1
[0089] The method is basically the same as Example 1, except that aluminum isopropoxide and n-butyl titanate are not added during the reaction to obtain polysiloxane.
[0090] Comparative Example 2
[0091] The method is basically the same as Example 1, except that no n-butyl titanate is added during the reaction to obtain polysiloxane.
[0092] Embodiment 3-5
[0093] The present embodiments provide an inorganic pigment, which is prepared by reacting a pigment base with a fluorosilane coupling agent, wherein the pigment base is a cadmium red pigment, and the preparation method thereof comprises:
[0094] In a 500mL three-necked flask equipped with a stirring paddle and a reflux condenser, add 15g of cadmium red pigment dried under vacuum at 180°C for 24h, a fluorosilane coupling agent (perfluorooctyl triethoxysilane / or tridecafluorooctyl triethoxysilane / or perfluorodecyl triethoxysilane) accounting for about 10% of the mass percentage of the cadmium red pigment, and 20 times the amount of reflux xylene used for the cadmium red pigment. Heat to about 85°C, drip the catalyst trifluoroacetic acid in the formula within 30min, heat to 115°C and reflux for more than 4h. Then filter out the cadmium red pigment, remove the solvent and excess ungrafted fluorosilane coupling agent, dry in a vacuum oven at 120°C for 2h, seal and leave for reuse, and obtain the raw materials and amounts used in Examples 3-5 as shown in Table 3.
[0095] Table 3
[0096]
[0097] Among them, the inorganic pigment prepared in Example 3 is referred to as fluorosilicone surface modified cadmium red pigment I, the inorganic pigment prepared in Example 4 is referred to as fluorosilicone surface modified cadmium red pigment II, and the inorganic pigment prepared in Example 5 is referred to as fluorosilicone surface modified cadmium red pigment III.
[0098] Application Example 1
[0099] This embodiment provides a polyurea composition and a preparation method thereof. The polyurea composition includes an isocyanate component and an amino compound component, and the mass ratio of the two components is 1:1. Among them, the raw material formula of the isocyanate component is shown in Table 4.
[0100] Table 4
[0101]
[0102] The route for synthesizing the prepolymer by hybridizing nano-titanium dioxide with polyaluminum titanium siloxane, hydroxyl-terminated polyether polyol and MDI-50 is as follows:
[0103]
[0104] Among them, the terminal hydroxyl groups present in the nano-titanium dioxide hybrid polyaluminum titanium siloxane can react with the terminal isocyanate groups in MDI-50, and other terminal isocyanate groups in MDI-50 can react with the hydroxyl groups of the terminal hydroxyl polyether polyol, thereby forming the structure shown above. Of course, the above only exemplifies one reaction connection method, and any terminal isocyanate group may react and connect with other terminal hydroxyl groups. The above exemplary process is only to more clearly show that the nano-titanium dioxide hybrid polyaluminum titanium siloxane of the present invention can be in-situ polymerized into the polyurea molecular structure.
[0105] Using the formula shown in Table 4, the preparation method of the isocyanate component includes: adding a formula amount of nano-titanium dioxide hybrid polyaluminum titanium siloxane, terminal hydroxyl polyether polyol and reflux xylene to a 500mL four-necked flask equipped with a stirring paddle and a reflux condenser, reflux dehydration at 140°C for 60min, cooling to 85°C, and then dripping the formula amount of MDI-50 within 30min. After the dripping, rinse the remaining material in the dropper bottle with 10mL of xylene, and then reflux at 90°C for 3h under nitrogen until the NCO content reaches the requirement, and then add the formula amount of inorganic pigment, and finally distill off the xylene and the low molecular weight products generated by the reaction under reduced pressure at 100±5°C and a vacuum degree of 0.095MPa, cool to room temperature, and obtain the isocyanate component, which is sealed and stored for use.
[0106] The raw material formula of the amino compound component is shown in Table 5.
[0107] Table 5
[0108]
[0109] The preparation method of the amino compound component comprises: adding a formulated amount of amino-terminated polyether and an amine chain extender into a 500 mL three-necked flask equipped with a stirring paddle, stirring at 5° C. until the components are evenly mixed, and sealing and storing for later use.
[0110] When applying: mix the isocyanate component and the amino compound component according to the feed ratio, and apply it by spraying. After the two components are mixed, the reaction process of the prepolymer and the amino-terminated polyether is shown as follows:
[0111]
[0112] The above process is only an exemplary description for ease of understanding. During the reaction process, the terminal amino group in the amino compound may react with any terminal isocyanate group.
[0113] Application Example 2
[0114] The same as the application example 1, the only difference is:
[0115] The raw material formula of the isocyanate component is shown in Table 6.
[0116] Table 6
[0117]
[0118]
[0119] The raw material formula of the amino compound component is shown in Table 7.
[0120] Table 7
[0121]
[0122] Application Example 3
[0123] The same as the application example 1, the only difference is:
[0124] The raw material formula of the isocyanate component is shown in Table 8.
[0125] Table 8
[0126]
[0127] The raw material formula of the amino compound component is shown in Table 9.
[0128] Table 9
[0129]
[0130]
[0131] Application Example 4
[0132] The same as the application example 1, the only difference is:
[0133] The raw material formula of the isocyanate component is shown in Table 10.
[0134] Table 10
[0135]
[0136] The raw material formula of the amino compound component is shown in Table 11.
[0137] Table 11
[0138]
[0139] Application Example 5
[0140] The same as the application example 1, the only difference is:
[0141] The raw material formula of the isocyanate component is shown in Table 12.
[0142] Table 12
[0143]
[0144]
[0145] The raw material formula of the amino compound component is shown in Table 13.
[0146] Table 13
[0147]
[0148] Application Example 6
[0149] The same as the application example 1, the only difference is:
[0150] The raw material formula of the isocyanate component is shown in Table 14.
[0151] Table 14
[0152]
[0153] The raw material formula of the amino compound component is shown in Table 15.
[0154] Table 15
[0155]
[0156] Application Comparative Example 1
[0157] It is basically the same as Application Example 1, except that: the nano titanium dioxide hybrid polyaluminum titanium siloxane is not added to the raw materials of the isocyanate component, and the fluorosilicon surface modified cadmium red pigment I is replaced by an untreated cadmium red pigment.
[0158] Application Comparative Example 2
[0159] It is basically the same as Application Example 1, except that the nano-titanium dioxide hybrid polyaluminum titanium siloxane in the raw material of the isocyanate component is replaced by the polysiloxane prepared in Comparative Example 1, and the fluorosilicon surface modified cadmium red pigment I is replaced by an untreated cadmium red pigment.
[0160] Application Comparative Example 3
[0161] It is basically the same as Application Example 1, except that the nano-titanium dioxide hybrid polyaluminum titanium siloxane in the raw material of the isocyanate component is replaced by the polysiloxane prepared in Comparative Example 2, and the fluorosilicon surface modified cadmium red pigment I is replaced by an untreated cadmium red pigment.
[0162] Performance Testing
[0163] The following performance tests were performed on the products obtained from Application Examples 1-6 and Comparative Examples 1-3. The specific results are shown in Table 16.
[0164] Table 16
[0165]
[0166] Test standard:
[0167] Gel time / s: GB / T15022.2-2007; Tensile strength: GB / T16777-2008; Tear strength: GB / T16777-2008; Adhesion (steel): GB / T31586.1-2015; Water absorption: GB / T15022.2-2007; Salt spray resistance (2000h): GB / T 1771-1991; Oil resistance: GB / T 9274-1988; Hardness: GB / T6739-2006; Impact strength: GB / T20624.2-2006; Heat resistance index: GB / T15022.2-2007; Limiting oxygen index LOI: GB / T2406.2-2009; Contact angle with water: GB / T24368-2009.
[0168] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
[0169] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
Claims
1. A polyurea composition comprising an isocyanate component and an amino compound component, characterized in that: The isocyanate component comprises a prepolymer and an inorganic pigment, wherein the raw materials of the prepolymer include: polyisocyanate, polyol, and nano-titanium dioxide hybrid polyaluminum titanium siloxane represented by formula (I); (Ⅰ); Wherein, X1, X2, X3, X4, and X5 are independently selected from the following groups: , , , , , , ; and there are terminal hydroxyl groups in X1, X2, X3, X4, and X5, and any two of them are not repeated, and at least , , one of the; t1, t2, t3, t4, t5 are independently selected from 0-100, and are not 0 when the corresponding group contains aluminum or titanium; R1, R2, R3, R4, R5, R6, R7, R8, and R9 are independently selected from C 1-20 Alkyl, phenyl, C 1-6 Alkyl-substituted phenyl, C 2-10 alkenyl; M is titanium dioxide, which is connected to silicon hydroxyl group, aluminum hydroxyl group or titanium hydroxyl group through hydrogen bonds via hydroxyl groups on the surface.
2. The polyurea composition according to claim 1, characterized in that: In formula (I), t1, t2, t3, t4 and t5 are independently selected from 0-50.
3. The polyurea composition according to claim 2, characterized in that: In formula (I), t1, t2, t3, t4 and t5 are independently selected from 0-30.
4. The polyurea composition according to claim 3, characterized in that: In formula (I), t1, t2, t3, t4 and t5 are independently selected from 0-20.
5. The polyurea composition according to claim 1, characterized in that: In formula (I), R1, R2, R3, R4, R5, R6, R7, R8 and R9 are independently selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, n-pentyl, isopentyl, neopentyl, n-hexyl, phenyl, C 1-6 Alkyl-substituted phenyl, vinyl, methyl vinyl, ethyl vinyl, propyl vinyl.
6. The polyurea composition according to claim 1, characterized in that: The average molecular weight of the nano titanium dioxide hybrid polyaluminum titanium siloxane represented by formula (I) is 500-10000.
7. The polyurea composition according to claim 6, characterized in that: The average molecular weight of the nano titanium dioxide hybrid polyaluminum titanium siloxane represented by formula (I) is 800-8000.
8. The polyurea composition according to claim 7, characterized in that: The average molecular weight of the nano titanium dioxide hybrid polyaluminum titanium siloxane represented by formula (I) is 1000-5000.
9. The polyurea composition according to claim 1, characterized in that: The mass ratio of the polyol to the nano-titanium dioxide hybrid polyaluminum titanium siloxane represented by formula (I) is 2-10:1; and / or the polyol is a hydroxyl-terminated polyether polyol.
10. The polyurea composition according to claim 1, characterized in that: The mass percentage of the isocyanate group of the prepolymer is 5%-20%.
11. The polyurea composition according to claim 1, characterized in that: The inorganic pigment is prepared by reacting a pigment matrix with a fluorosilane coupling agent, wherein the fluorosilane coupling agent comprises at least one of perfluorooctyltriethoxysilane, tridecafluorooctyltriethoxysilane and perfluorodecyltriethoxysilane.
12. The polyurea composition according to claim 1, characterized in that: The amino compound component comprises polyoxypropylene diamine and selectively comprises at least one of 3,5-diethyl-2,4-diaminotoluene, 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, 4,4'-diaminodicyclohexylmethane and 4,4'-bis-sec-butylaminodiphenylmethane; and / or, the feed mass ratio of the isocyanate component to the amino compound component is 1:0.5-2.
13. A method for preparing the polyurea composition according to any one of claims 1 to 12, characterized in that: The preparation method comprises a preparation process of an isocyanate component, wherein the preparation process of the isocyanate component comprises: mixing and reacting polyisocyanate, polyol and nano titanium dioxide hybrid polyaluminum titanium siloxane represented by formula (I) to generate a prepolymer, and then mixing the prepolymer with an inorganic pigment.
14. Use of the polyurea composition according to any one of claims 1 to 12 in anti-corrosion materials.
Citation Information
Patent Citations
Polyureas copolymer with main chain containing siloxane composition unit and preparation method thereof
CN103834034A
Hybridized hard-segment material modified elastomer material and preparation method thereof
CN109942782A
Water-based resin paint
CN112778866A
Marine nontoxic antifouling organosilicon modified polyurea and preparation method thereof
CN112794975A
Composition and process for preparing silylated polymers, and use thereof
CN113631606A