High reflectivity PBT composition suitable for making reflective cups and its preparation and application

By blending PBT with PET, blending special-shaped glass fiber and whisker reinforcement in reflective cup material, filling with chlorinated titanium dioxide and high-white ceramic microbeads, combined with flame retardant, the reflectivity of existing reflective cup materials is solved. The problems of low and poor heat dissipation have achieved the improvement of high reflectivity and good heat dissipation efficiency, and are suitable for the secondary light distribution and heat dissipation needs of LED downlights.

CN115895201BActive Publication Date: 2024-11-26CGN TOXXON (XIAMEN) NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211257071.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-14
Publication Date
2024-11-26
Estimated Expiration
2042-10-14

AI Technical Summary

Technical Problem

The existing reflective cup materials have problems such as low reflectivity, poor heat dissipation, complex processing, high cost and unstable performance in LED downlights. Especially under high temperature conditions, the materials are prone to degradation, resulting in reduced light efficiency and shortened lifetime.

Method used

Using a high reflectivity PBT composition, blending PBT with PET, blending with PBT, shaped glass fiber and whisker reinforcement, chlorinated titanium dioxide and high whiteness ceramic microbeads, combined with bromine system and synergistic flame retardant, to form a high reflectance Material system with good heat dissipation, stability and low cost.

Benefits of technology

It achieves a reflectivity of more than 95%, improves the stability of the material and heat dissipation efficiency, reduces the amount of warping and deformation, ensures the dimensional stability of the parts and the light source utilization rate, and is suitable for the production of reflective cups in high-temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115895201B_ABST
    Figure CN115895201B_ABST
Patent Text Reader

Abstract

The invention discloses a high-reflectivity PBT composition suitable for making a reflective cup. The raw material composition includes, by weight, 30 to 50 parts of PBT resin, 10 to 20 parts of PET resin, 5 to 8 parts of shaped glass fiber, 5 to 10 parts of whisker, 4 to 7 parts of toughening and compatibilizing agent, 8 to 14 parts of flame retardant, 20 to 30 parts of reflective filling mineral, and 0.8 to 1.5 parts of processing aid. The preparation method includes: mixing PBT resin, PET resin, toughening and compatibilizing agent, flame retardant, reflective filling mineral, and processing aid uniformly, and then feeding into the main feeding port of a twin-screw extruder, and the shaped glass fiber and whisker are added from two side feeding ports in the middle of the twin-screw extruder respectively, and the temperature of the twin-screw extruder is controlled at 180 to 240° C. After mixing and plasticizing, the molten material is extruded and granulated to obtain high-reflectivity PBT composition plastic particles. The high-reflectivity PBT composition of the invention can be used to make a reflective cup.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polybutylene terephthalate (PBT) compositions, and in particular to a high-reflectivity PBT composition suitable for making a reflective cup, and a preparation method and application thereof. Background Art

[0002] As one of the main components of lamps, reflective cups play an important role. In LED downlights, the main function of reflective cups is to serve as a secondary light distribution reflective structure, improve the glare of the lamp, and make the light-emitting surface emit light evenly and softly. In addition, since the reflective cup has a trumpet-shaped opening close to the lamp beads, the lamp beads will emit a lot of heat when they are lit. When the heat cannot be well conducted and dissipated, it is easy to cause the operating temperature of the lamp to rise, further reduce the light efficiency of the light source, accelerate the light decay of the lamp beads, and shorten the life. Therefore, in addition to the light distribution function, the reflective cup also needs to have a certain heat dissipation function.

[0003] The material of the early LED downlight reflector cup is metal aluminum, which has good heat dissipation effect, but the reflectivity of light is relatively low, and the metal is not easy to process and the cost is high. Subsequent reflector cups use aluminum-plated PC plastics as the reflective layer. Although it is easy to form reflective cups of various shapes, it requires an additional aluminum plating process. Now reflective PC plastic materials are gradually used to directly inject and mold reflective cups. For example, Chinese patent application CN103435995A discloses a high-light-blocking and high-reflective PC, and its material uses a high content of titanium dioxide to fill (10-20%) to improve the reflectivity. For example, Chinese patent application CN114213829A discloses a flame-retardant, light-blocking and highly reflective PC material, which uses a reflective component composed of PC resin, titanium dioxide, hollow structure ultrafine glass powder and coupling agent with a mass ratio of 45: (25-45): (15-40): (5-20) with a mass ratio of up to 25-70%. In actual injection molding, high content of titanium dioxide under high temperature conditions of barrel and hot runner can easily induce partial degradation of polycarbonate, making the material brittle and producing material flowers on the surface of the injection molded part, which reduces the reflectivity of the reflective cup. Reflective cups made of highly reflective PC materials have quality stability fluctuations and general heat dissipation effects.

[0004] In view of the technical defects of the above materials, the present invention develops a PBT composition with stable performance and high reflectivity for use in injection-molded reflective cups to solve the problems of secondary light distribution of downlights and poor heat dissipation of lamp beads. Summary of the invention

[0005] The invention provides a high-reflectivity PBT composition suitable for making a reflective cup, which has excellent reflectivity, the reflectivity reaches more than 95% (at555nm), and the injection molding processing performance is stable and reliable, which meets the light distribution requirements of the reflective cup of the lamp, and has insulation, flame retardancy and heat dissipation functions, and solves the problems of complex processing, high cost, poor heat dissipation, and unstable and controllable reflectivity and mechanical strength performance of current reflective materials during mass production.

[0006] A high-reflectivity PBT composition suitable for making a reflective cup, wherein the raw materials include, by weight:

[0007]

[0008] The intrinsic viscosity of the PBT resin is 0.8 to 0.9 dL / g, preferably 0.80 to 0.83 dL / g, and more preferably 0.80 dL / g;

[0009] The intrinsic viscosity of the PET resin is 0.65 to 0.85 dL / g, preferably 0.8±0.015 dL / g, and more preferably 0.80 dL / g;

[0010] The whiskers are one or more of aluminum oxide, zinc oxide, calcium sulfate, silicon carbide, boron nitride, aluminum borate, and ceramic whiskers, preferably at least one of zinc oxide and boron nitride whiskers;

[0011] The reflective filling mineral is one or more of titanium dioxide, glass microbeads, ceramic microbeads, barium sulfate, and zinc sulfide, preferably a compound mixture of chloride titanium dioxide and high-whiteness solid ceramic microbeads, the whiteness of the high-whiteness solid ceramic microbeads is above 95, and further preferably, the amount of chloride titanium dioxide in the compound mixture is greater than the high-whiteness solid ceramic microbeads. Chloride titanium dioxide has strong covering power and high intensity of reflected light, and is not easy to cause material degradation in the polyester material system, and the processing stability is more reliable. High-whiteness solid ceramic microbeads have a smooth and hard surface, anti-warping, inhibit glass fiber exposure, and a whiteness of above 95. Improving the smoothness and flatness of the material surface is conducive to light reflection.

[0012] The high reflectivity PBT composition of the present invention has the following characteristics:

[0013] 1. When PBT is blended with PET, the crystallization speed slows down, and the thickness of the amorphous layer on the surface of the material increases during molding, so that the material has the characteristics of good surface gloss and small deflection, which is conducive to the reflection of light.

[0014] 2. Use a small amount of special-shaped glass fiber and whisker to replace ordinary glass fiber as a reinforcing agent to improve the mechanical properties, heat resistance, and dimensional stability of the material, avoid warping caused by inconsistent longitudinal and transverse shrinkage rates of the parts due to glass fiber orientation, and reduce the impact on the surface gloss of the material and improve the light reflectivity. At the same time, boron nitride whiskers can further improve the thermal conductivity of PBT materials to achieve a better heat dissipation effect.

[0015] 3. Chloride-process rutile titanium dioxide and high-whiteness solid ceramic microbeads are compounded and filled with PBT / PET substrate. The material has extremely high opacity and optimal whiteness and brightness. Reasonable proportions can make the reflectivity of the material surface to visible light reach more than 95%.

[0016] In a preferred example, the terminal carboxyl group of the PBT resin is ≤24 mol / t.

[0017] In a preferred example, the special-shaped glass fiber is one or more of alkali-free glass fiber, medium-alkali glass fiber, and high-strength glass fiber.

[0018] In a preferred example, the monofilament diameter of the shaped glass fiber is 7-17 μm, and the chopped length of the glass strand is 1.7-4.5 mm.

[0019] Furthermore, the shaped glass fiber is preferably a short-cut alkali-free glass fiber with a diameter of 10 to 17 μm, a short length of the glass strands of 3 to 4.5 mm, and a flattened cross-sectional shape.

[0020] Furthermore, the shaped glass fiber is preferably a short-cut alkali-free glass fiber with a diameter of 13 to 17 μm, a short length of the glass strand of 3 mm, and a shape structure of a flattened cross-section with a shape ratio of (3±0.3):1.

[0021] The shaped glass fibers are preferably added by side feeding to maintain effective reinforcement length and structural shape.

[0022] The whiskers are preferably added by side feeding to reduce excessive shearing and maintain a limited aspect ratio.

[0023] The toughening and compatibilizing agent can be one or more of maleic anhydride grafted ethylene and octene copolymer (POE grafted MAH), polyester elastomer, polyolefin elastomer, ethylene-methyl acrylate, ethylene-butyl acrylate, ethylene-acrylate-GMA terpolymer (such as AX8750, etc.), preferably Arkema AX8750, which has high fluidity and ester content, ensuring that the PBT material meets the requirements of molding thin-walled reflective cup parts while having high material toughness.

[0024] In a preferred example, the flame retardant is compounded by a brominated flame retardant and a synergistic flame retardant.

[0025] The brominated flame retardant may be at least one of brominated polystyrene, brominated epoxy resin, decabromodiphenylethane, and phenoxytetrabromobisphenol A carbonate oligomer (such as BC52, BC58, etc.).

[0026] The synergistic flame retardant may be at least one of antimony trioxide, zinc borate, and sodium antimonate.

[0027] The flame retardant is preferably compounded from at least one of brominated epoxy resin and phenoxy tetrabromobisphenol A carbonate oligomer (such as BC52, BC58, etc.) and antimony trioxide in a mass ratio of 2 to 5: 1. The flame retardant system has higher temperature resistance in PBT materials, reducing appearance problems such as black lines, yellow lines, and carbonization during high-temperature processing.

[0028] The processing aid may be one or more of a primary antioxidant, a secondary antioxidant, an internal lubricant, and an external lubricant.

[0029] The primary antioxidant may be one or more of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, triethylene glycol bis[β-(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate] (antioxidant 245), β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, and 1,3,5-tris(4-tert-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione.

[0030] The auxiliary antioxidant may be one or more of tris[2.4-di-tert-butylphenyl]phosphite, bis(2,4-di-tert-butylphenol)pentaerythritol diphosphite (antioxidant 626), bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphate, and pentaerythritol tetrakis(3-laurylthiopropionate).

[0031] The internal lubricant is one or more of montan wax, polyethylene wax and zinc stearate.

[0032] The external lubricant is a silicone lubricant and / or pentaerythritol stearate.

[0033] The present invention also provides a method for preparing the high-reflectivity PBT composition, comprising: uniformly mixing PBT resin, PET resin, toughening and compatibilizing agent, flame retardant, reflective filling mineral and processing aid, and then feeding into the main feeding port of a twin-screw extruder, and adding the shaped glass fiber and whisker from two side feeding ports in the middle of the twin-screw extruder respectively, and the temperature of the twin-screw extruder is controlled at 180-240° C. After mixing and plasticizing, the molten material is extruded and granulated to obtain high-reflectivity PBT composition plastic particles.

[0034] In a preferred example, in the preparation method, the side feeding ports of the shaped glass fibers and whiskers are respectively located upstream and downstream of the twin-screw extruder.

[0035] In a preferred example, in the preparation method, the PBT resin, PET resin, toughening and compatibilizing agent, flame retardant, reflective filling mineral and processing aid are uniformly mixed for 1.5 to 2 minutes using a high-speed mixer.

[0036] In a preferred example, in the preparation method, the main engine speed of the twin-screw extruder is 350-400 rpm.

[0037] The present invention also provides the use of the high-reflectivity PBT composition in making a reflective cup. The reflective cup can be used as a secondary light distribution structural component of an LED downlight or other lamps to reduce light loss and improve light source utilization.

[0038] As a general inventive concept, the present invention also provides a reflective cup, which is obtained by injection molding using the high-reflectivity PBT composition or the high-reflectivity PBT composition plastic particles prepared by the preparation method as raw materials.

[0039] Compared with the prior art, the present invention has the following beneficial effects:

[0040] 1) Use special-shaped glass fiber and whisker reinforcement to improve the strength of the material, and the heat deformation temperature can reach above 160°C, which can meet the long-term use of the reflective cup in a high-temperature environment, reduce the warping deformation of the PBT composition, and ensure the dimensional stability of the product. At the same time, boron nitride whiskers and reflective filling minerals can increase the thermal conductivity of the PBT resin substrate to 0.5W / m / K, and the heat dissipation efficiency of the material is improved.

[0041] 2) Chloride-process titanium dioxide and high-whiteness solid ceramic microbeads compounded with filling minerals can give PBT extremely high opacity, whiteness, and surface brightness, with a reflectivity of more than 95%.

[0042] 3) Adding low-viscosity PET resin to low-viscosity PBT resin can inhibit the crystallization of the material, increase the thickness of the amorphous layer on the surface, significantly increase the surface gloss of the material, further improve the surface reflectivity, and the material has excellent fluidity and can be formed into reflective cup parts with different thickness requirements. The material system has high temperature resistance, a wide processing temperature range, low cost, and is easy to apply and promote in the market. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 This is a photo of the LED downlight reflector cup manufactured in Example 6. DETAILED DESCRIPTION

[0044] The present invention will be further described below in conjunction with the accompanying drawings and specific examples. It should be understood that these examples are only intended to illustrate the present invention and are not intended to limit the scope of the present invention. The operating methods in the following examples without specifying specific conditions are usually carried out under conventional conditions or under conditions recommended by the manufacturer.

[0045] Each embodiment and comparative example of the present invention is injection molded into corresponding standard specimens according to standard requirements and tested. Among them, the tensile strength is in accordance with GB / T 1040 standard; the bending strength and bending modulus are in accordance with GB / T 9341 standard; the cantilever beam notched impact strength is in accordance with GB / T 1843 standard; the thermal conductivity is in accordance with ASTM-E1461 standard; the heat deformation temperature is in accordance with GB / T 1634 standard; the flame retardant test is in accordance with UL94 standard; the total light reflectivity is tested by Datacolor 200M optical instrument, and the reflectivity corresponding to the wavelength of at555nm is used as the characterization data. The test standard sample size is a flat color plate injection molded part with a thickness of 2mm and a length and width of 60mm; the warpage deformation evaluation test is performed by injecting the material into a square flat plate with a thickness of 1mm and a side length of 100mm with a single port injection, cooling at 23℃ for 24 hours, and placing it on a glass horizontal surface. The maximum gap between the flat plate and the glass horizontal surface is measured with a plug gauge as the warpage deformation.

[0046] The raw materials used in the embodiments and comparative examples of the present invention are as follows:

[0047] PBT resin: PBTKH2080 (intrinsic viscosity 0.80 dL / g), PBTKH2100 (intrinsic viscosity 1.0 dL / g), Yingkou Kanghui Petrochemical Co., Ltd.;

[0048] PET resin: high gloss water bottle grade PET BG80 (intrinsic viscosity 0.80dL / g), PET BG85 (intrinsic viscosity 0.88dL / g), Sinopec Yizheng Chemical Fiber Co., Ltd.;

[0049] Glass fiber: PBT modified special shaped chopped glass fiber ECS303A-3-M3, effective monofilament diameter 15-17μm, short side monofilament diameter 8±1μm, chopped length 3mm, profile ratio 3±0.3, Chongqing International Composite Materials Co., Ltd.; PBT modified special ordinary chopped glass fiber ECS17-4.5-534A, monofilament diameter 17μm, chopped length 4.5mm, China Jushi Co., Ltd.

[0050] Whiskers: Tetrapod-shaped zinc oxide whiskers, diameter 0.5-5 μm, length 10-50 μm, Hangzhou Jikang New Materials Co., Ltd.; Boron nitride whiskers, hexagonal crystal, diameter 1-3 μm, aspect ratio 10-100, Zhejiang Yamei Nanotechnology Co., Ltd.;

[0051] Toughening and compatibilizing agent: AX8750 (GMA terpolymer), Arkema, France;

[0052] Compound flame retardant: brominated epoxy resin CXB-2000H (bromine content: 53% molecular weight: 20000), South Korea's Yujin; brominated aromatic flame retardant BC 58 (bromine content: 58% molecular weight: 973), Germany's Lanxess; antimony trioxide (Sb2O3≥99.90%), Guangdong Yuxing Flame Retardant New Materials Co., Ltd.

[0053] Reflective filling minerals: Chloride titanium dioxide CR-834, American Trono (Kemeiji); High whiteness solid ceramic microspheres HG-T, Shanghai Huijingya Nano New Materials Co., Ltd.; Precipitated barium sulfate AY-F300 (whiteness ≥ 98%), Foshan Anyi Nano Materials Co., Ltd.

[0054] Processing aids: antioxidant Irganox 245 (hindered phenol), BASF, Germany; antioxidant 626 (organic phosphite), SI Group; polyethylene wax AClyn 295, Honeywell; silicone lubricant E525, Evonik, Germany.

[0055] Examples 1 to 6

[0056] A method for preparing a high-reflectivity PBT composition suitable for making a reflective cup of a lamp comprises the following steps:

[0057] (1) Weigh the raw materials according to the weight proportions of PBT resin, PET resin, toughening and compatibilizing agent, compound flame retardant (brominated flame retardant and antimony trioxide), titanium dioxide, solid ceramic microspheres, and various processing aids in Table 1;

[0058] (2) adding the weighed raw materials of each component in step (1) into a high-speed mixer and mixing for 1.5 minutes to prepare a premix;

[0059] (3) The premix is ​​added to the main feed port of the twin-screw extruder in proportion by weight loss weighing, the special-shaped glass fiber is added by the first-stage side feeder of the fifth barrel by weight loss weighing, and the whisker is added by the second-stage side feeder of the eighth barrel by weight loss weighing. The length-to-diameter ratio of the twin-screw extruder is 48:1, with a total of twelve sections. The natural exhaust port is located in the fourth and seventh sections, and the vacuum exhaust port is located in the eleventh section. The screw combination adopts medium shear and strong dispersion. All materials are melted, plasticized, and extruded into granules by the twin-screw extruder. Among them, the speed of the twin-screw extruder is 380rpm, and the temperature distribution from the feed section to the die head is: 200℃, 240℃, 240℃, 240℃, 220℃, 220℃, 200℃, 200℃, 180℃, 180℃, 180℃, die head: 240℃, after extrusion, the material is water-cooled, dried, pelletized, mixed evenly, and then packaged.

[0060] Preparation of test standard samples: The modified plastic pellets were placed in a forced air drying oven and dried at 110°C for 4 hours, and then molded by an injection molding machine to prepare test specimens, flat color plates, and square flat plates. The performance test results of Examples 1 to 6 are shown in Table 2.

[0061] Table 1 Weight parts of each raw material in Examples 1 to 6

[0062]

[0063] Table 2 Performance test results of Examples 1 to 6

[0064]

[0065] Comparative Examples 1 to 7

[0066] Comparative Examples 1 to 7: After weighing the raw materials (excluding glass fiber and whisker) according to the weight of each material in Table 3, a high reflectivity PBT composite material was prepared according to the method of step (2) and step (3) of the above embodiment. The obtained modified PBT composite material was placed in a blast drying oven and dried at 110° C. for 4 hours, and then molded by an injection molding machine to prepare test specimens, flat color plates, and square flat plates. The performance test results of Comparative Examples 1 to 7 are shown in Table 4.

[0067] Table 3 Weight parts of each raw material in Comparative Examples 1 to 7

[0068]

[0069] Table 4 Performance test results of comparative examples 1 to 7

[0070]

[0071] By comparing Comparative Example 1 with Example 1, it can be seen that the use of flattened shaped glass fibers can significantly reduce the warping deformation of the PBT composite material, and the mechanical strength is not much different from that of ordinary round glass fiber reinforcement.

[0072] By comparing Comparative Example 2 with Example 3, it can be seen that the reflective filling mineral selected by titanium dioxide and ceramic microbeads compounded with PBT material has a higher reflectivity, and under the same filling ratio conditions, titanium dioxide compounded with ultra-white precipitated barium sulfate cannot achieve a higher reflectivity. By comparing Comparative Example 3 and Comparative Example 4 with Example 3, it can be seen that when all ceramic microbeads or all titanium dioxide are used as reflective filling minerals, the reflectivity of the material is lower than 93%. The high-filling titanium dioxide has better light reflection ability than ceramic microbeads, so it is used as the main body of reflective filling minerals. Ceramic microbeads have a regular spherical shape and a smooth and hard surface. The PBT resin substrate is evenly dispersed on the surface of the material after high-temperature melting and plasticization. The compounded titanium dioxide has very high opacity, glossiness, and whiteness, which makes the surface of the PBT material have ultra-high reflectivity to light.

[0073] By comparing Comparative Example 5 with Example 6, it can be seen that the addition of PET resin can significantly improve the light reflectivity of the PBT composite material. PBT has a fast crystallization speed, while PET has a slow crystallization speed. When the two are blended, the crystallization speed slows down, which will increase the thickness of the amorphous layer on the surface of the molded product and improve the surface gloss. In addition, the low-viscosity PET and PBT resins used in the formula system have high fluidity and have a better wrapping effect on a small amount of glass fiber, so the reflectivity of the surface of the PBT composite material is higher. By comparing Comparative Example 6 with Example 6, it can be seen that the reinforcement of a small amount of wave fibers significantly improves the mechanical properties and heat deformation temperature of the PBT composite material. It is difficult to improve the mechanical strength and heat deformation temperature of the material by replacing all of them with whiskers as a reinforcing agent. However, the increase in glass fiber content will reduce the reflectivity of the material surface. Therefore, the flattened glass fiber content is reasonably controlled at 5 to 8 parts by weight to take into account the performance and reflectivity performance requirements.

[0074] By comparing Comparative Example 7 with Example 6, it can be found that the material using the low-viscosity PBT / PET resin compound as the substrate has a higher reflectivity than the high-viscosity PBT / PET resin compound as the substrate. The low-viscosity resin has higher fluidity, which is beneficial to the die and has a higher surface brightness.

[0075] Figure 1 The actual photo of the LED downlight reflector cup manufactured in Example 6 is shown.

[0076] In addition, it should be understood that after reading the above description of the present invention, those skilled in the art may make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims attached to this application.

Claims

1. A high reflectivity PBT composition suitable for making a reflective cup, characterized in that: By weight, the raw material composition includes: The intrinsic viscosity of the PBT resin is 0.8 to 0.9 dL / g; The intrinsic viscosity of the PET resin is 0.8±0.015 dL / g; The whiskers are boron nitride whiskers; The reflective filling mineral is a compound mixture of chloride titanium dioxide and high-whiteness solid ceramic microspheres, the whiteness of the high-whiteness solid ceramic microspheres is above 95; the amount of chloride titanium dioxide in the compound mixture is greater than that of the high-whiteness solid ceramic microspheres.

2. The high reflectivity PBT composition according to claim 1, characterized in that: The intrinsic viscosity of the PBT resin is 0.80 to 0.83 dL / g.

3. The high reflectivity PBT composition according to claim 1, characterized in that: The terminal carboxyl group of the PBT resin is ≤24 mol / t.

4. The high reflectivity PBT composition according to claim 1, characterized in that: The special-shaped glass fiber is one or more of alkali-free glass fiber, medium-alkali glass fiber, and high-strength glass fiber; The monofilament diameter of the special-shaped glass fiber is 7-17 μm, and the short length of the glass raw fiber is 1.7-4.5 mm.

5. The high reflectivity PBT composition according to claim 4, characterized in that: The special-shaped glass fiber has a diameter of 10 to 17 μm, a short-cut length of the glass raw fiber of 3 to 4.5 mm, and a body structure of a short-cut alkali-free glass fiber with a flattened cross-section shape.

6. The high reflectivity PBT composition according to claim 1, characterized in that: The toughening and compatibilizing agent is one or more of maleic anhydride grafted ethylene and octene copolymer, polyester elastomer, polyolefin elastomer, ethylene-methyl acrylate, ethylene-butyl acrylate, and ethylene-acrylate-GMA terpolymer.

7. The high reflectivity PBT composition according to claim 6, characterized in that: The toughening and compatibilizing agent is Arkema AX8750.

8. The high reflectivity PBT composition according to claim 1, characterized in that: The flame retardant is compounded by a brominated flame retardant and a synergistic flame retardant; The brominated flame retardant is at least one of brominated polystyrene, brominated epoxy resin, decabromodiphenylethane, and phenoxy tetrabromobisphenol A carbonate oligomer; The synergistic flame retardant is at least one of antimony trioxide, zinc borate and sodium antimonate.

9. The high reflectivity PBT composition according to claim 8, characterized in that: The flame retardant is prepared by compounding at least one of brominated epoxy resin and phenoxy tetrabromobisphenol A carbonate oligomer with antimony trioxide in a mass ratio of 2 to 5:

1.

10. The high reflectivity PBT composition according to claim 1, characterized in that: The processing aid is one or more of a primary antioxidant, an auxiliary antioxidant, an internal lubricant, and an external lubricant; The primary antioxidant is one or more of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, triethylene glycol bis[β-(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate], β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, and 1,3,5-tris(4-tert-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione; The auxiliary antioxidant is one or more of tris[2,4-di-tert-butylphenyl]phosphite, bis(2,4-di-tert-butylphenol)pentaerythritol diphosphite, bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphate, and pentaerythritol tetrakis(3-laurylthiopropionate); The internal lubricant is one or more of montan wax, polyethylene wax, and zinc stearate; The external lubricant is a silicone lubricant and / or pentaerythritol stearate.

11. The method for preparing a high reflectivity PBT composition according to any one of claims 1 to 10, characterized in that: include: PBT resin, PET resin, toughening and compatibilizing agent, flame retardant, reflective filling mineral and processing aid are mixed evenly, and then fed into the main feeding port of a twin-screw extruder. Shaped glass fiber and whisker are respectively added from two side feeding ports in the middle of the twin-screw extruder. The temperature of the twin-screw extruder is controlled at 180-240° C. The molten material is mixed and plasticized and then extruded and granulated to obtain high-reflectivity PBT composite plastic particles.

12. Use of the high reflectivity PBT composition according to any one of claims 1 to 10 in making a reflective cup.

13. The use according to claim 12, characterized in that: The reflective cup is used as a secondary light distribution structural component of an LED downlight or other lamps.

14. A reflective cup, characterized in that: The reflective cup is obtained by injection molding using the high-reflectivity PBT composition according to any one of claims 1 to 10 or the high-reflectivity PBT composition plastic particles prepared by the preparation method according to claim 11 as raw materials.