Oxidized carbon nanotubes and method for producing the same
Oxidized carbon nanotubes with specific properties and production methods improve dispersibility and stability in water, addressing aggregation issues of CNTs, while maintaining conductivity and thermal properties.
Patent Information
- Application Number
- CN202180042453.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-08-28
- Filing Date
- 2021-07-29
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2041-07-29
AI Technical Summary
Existing carbon nanotube (CNT) dispersions face challenges in achieving uniform dispersibility and stability in water due to aggregation and entanglement, with prior methods like fibrous carbon nanostructure dispersions still requiring improvement.
Oxidized carbon nanotubes containing oxidized single-walled CNTs at a predetermined ratio, with specific properties such as a D' band in the Raman spectrum, oxygen atomic ratio, and BET specific surface area, are produced through controlled oxidation treatment using nitric acid to enhance dispersibility and stability.
The resulting oxidized CNTs exhibit excellent dispersibility and dispersion stability in water, maintaining electrical and thermal conductivity while preventing damage to their properties.
Smart Images

Figure BDA0003996303220000211 
Figure BDA0003996303220000212 
Figure BDA0003996303220000291
Abstract
Description
Technical Field
[0001] The present invention relates to oxidized carbon nanotubes and a method for producing the same. Background Art
[0002] Carbon nanotubes (hereinafter sometimes referred to as "CNTs") are excellent in various properties such as mechanical strength, optical properties, electrical properties, thermal properties, and molecular adsorption capacity, and are expected to be developed as functional materials such as electronic device materials, optical element materials, and conductive materials.
[0003] On the other hand, when using CNTs, they need to be uniformly dispersed in water in order to fully exert their properties. However, CNTs are easily aggregated and entangled with each other, making it difficult to uniformly disperse them.
[0004] Therefore, in recent years, technologies for improving the dispersibility of CNTs have been developed. For example, in Patent Document 1, a fibrous carbon nanostructure dispersion is proposed, which includes a fibrous carbon nanostructure such as CNT and a solvent, wherein the fibrous carbon nanostructure such as CNT has a wavelength of 500 cm-1 in the spectral absorption spectrum. -1 Over 600cm -1 The following wave number region has at least one absorption peak.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent document 1: International Publication No. 2018 / 180901. Summary of the invention
[0008] Problem that the invention aims to solve
[0009] However, the fibrous carbon nanostructure dispersion described in Patent Document 1 still has room for further improvement in terms of improving dispersibility and dispersion stability in water.
[0010] Therefore, an object of the present invention is to provide an oxidized carbon nanotube having excellent dispersibility and dispersion stability in water.
[0011] Another object of the present invention is to provide a method for producing oxidized carbon nanotubes having excellent dispersibility and dispersion stability in water.
[0012] Solutions for solving problems
[0013] The present inventors conducted intensive studies to solve the above problems and found that, among oxidized CNTs containing oxidized single-walled CNTs at a predetermined ratio, oxidized CNTs having predetermined properties are excellent in dispersibility and dispersion stability in water.
[0014] That is, the object of the present invention is to advantageously solve the above-mentioned problems, and the oxidized carbon nanotubes of the present invention are characterized in that they are oxidized carbon nanotubes containing oxidized single-walled carbon nanotubes, the number of the oxidized single-walled carbon nanotubes accounts for more than 50% of the total number of the oxidized carbon nanotubes, and the oxidized carbon nanotubes have a D' band in the Raman spectrum. As such, the oxidized CNTs containing oxidized single-walled CNTs at a predetermined ratio and having a D' band in the Raman spectrum have excellent dispersibility and dispersion stability in water.
[0015] It should be noted that, in the present invention, "oxidized CNT" refers to CNT having an oxygen atomic ratio of more than 4 at %. The oxygen atomic ratio of the oxidized CNT can be determined using the method described in Examples of this specification.
[0016] In the present invention, "the ratio of the number of oxidized single-walled CNTs to the total number of oxidized CNTs" can be determined using the method described in Examples of this specification.
[0017] Furthermore, in the present invention, the presence or absence of the "D' band" can be determined using the method described in the Examples of this specification.
[0018] Here, the oxidized carbon nanotubes of the present invention preferably have an average diameter of 3.5 nm to 5 nm. If the average diameter of the oxidized CNTs is 3.5 nm to 5 nm, the electrostatic repulsion between the oxidized CNTs increases, and the dispersibility of the oxidized CNTs can be improved.
[0019] In the present invention, the "average diameter of oxidized CNTs" can be determined using the method described in Examples of this specification.
[0020] In addition, the oxidized carbon nanotubes of the present invention preferably have an oxygen atomic ratio of 15 at % or more. When the oxygen atomic ratio of the oxidized CNTs is 15 at % or more, the electrostatic repulsion between the oxidized CNTs increases, thereby improving dispersibility.
[0021] Furthermore, the oxidized carbon nanotubes of the present invention preferably have an average length of 30 nm to 120 nm. If the average length of the oxidized CNTs is 30 nm to 120 nm, the dispersibility of the oxidized CNTs in water can be further improved.
[0022] In the present invention, the "average length of oxidized CNTs" can be obtained using the method described in Examples of this specification.
[0023] In addition, the present invention aims to advantageously solve the above-mentioned problems. The method for producing oxidized carbon nanotubes of the present invention is characterized in that it is the above-mentioned method for producing oxidized carbon nanotubes, comprising an oxidation treatment step of oxidizing carbon nanotubes including single-walled carbon nanotubes, wherein the BET specific surface area of the carbon nanotubes is greater than 1300 m 2 / g. In this way, by using single-walled CNTs with a BET specific surface area greater than 1300 m 2 By oxidizing CNTs of 100 μg / cm2, multiple edge portions can be formed on the surface of the CNTs. At the same time, by cutting the CNTs using these edge portions as starting points, oxidized CNTs can be efficiently produced.
[0024] In the present invention, the "BET specific surface area" refers to a nitrogen adsorption specific surface area measured using the BET method.
[0025] Here, in the method for producing oxidized carbon nanotubes of the present invention, it is preferred that the carbon nanotubes have a G / D ratio greater than 3.0 and less than 10. When CNTs having a G / D ratio greater than 3.0 and less than 10 are used, the dispersibility of the obtained oxidized CNTs can be improved.
[0026] In the present invention, the "G / D ratio" refers to the ratio of the intensity of the G band peak to the intensity of the D band peak in the Raman spectrum. The "G / D ratio" can be obtained using the method described in Examples of the present specification.
[0027] In addition, in the method for producing oxidized carbon nanotubes of the present invention, it is preferred that in the oxidation treatment step, the oxidation treatment is performed using an aqueous nitric acid solution having a concentration greater than 40% by mass. If the CNTs are oxidized using an aqueous nitric acid solution having a concentration greater than 40% by mass, the CNTs are cut shorter by increasing the number of edge portions formed on the surface of the CNTs, thereby further improving the dispersibility and dispersion stability of the obtained oxidized CNTs.
[0028] Furthermore, in the method for producing oxidized carbon nanotubes of the present invention, it is preferred that in the oxidation treatment step, the mixture containing the carbon nanotubes and the aqueous nitric acid solution is refluxed at a temperature of ±5°C of the azeotropic point of the aqueous nitric acid solution. If the mixture containing CNTs and the aqueous nitric acid solution is refluxed at a temperature of ±5°C of the azeotropic point of the aqueous nitric acid solution, the oxidation treatment can be sufficiently performed, and the production efficiency of oxidized CNTs can be further improved.
[0029] Furthermore, in the method for producing oxidized CNTs of the present invention, it is preferred that the carbon nanotubes are oxidized in the oxidation step so that the single-wall ratio change rate represented by the following formula (1) becomes 90% or less.
[0030] Single wall ratio change rate = SGCNT A / SGCNTB ×100(%)…Formula (1) It should be noted that in formula (1), SGCNT A It represents the ratio of the number of oxidized single-walled carbon nanotubes to the total number of oxidized carbon nanotubes. B It indicates the ratio of the number of single-walled carbon nanotubes to the total number of carbon nanotubes.
[0031] By performing the oxidation treatment so that the single-wall ratio change rate becomes 90% or less in this manner, the dispersibility and dispersion stability of the obtained oxidized CNT in water can be further improved.
[0032] In the present invention, "the ratio of the number of single-walled CNTs to the total number of CNTs" can be determined using the method described in Examples of this specification.
[0033] In the method for producing oxidized carbon nanotubes of the present invention, it is preferred that the carbon nanotubes are oxidized in the oxidation step so that the average diameter change rate represented by the following formula (2) is greater than 100%.
[0034] Average diameter change rate = CNT DA / CNT DB ×100(%)…Formula (2)
[0035] It should be noted that in formula (2), CNT DA represents the average diameter of oxidized carbon nanotubes, CNT DB represents the average diameter of carbon nanotubes.
[0036] By performing the oxidation treatment so that the average diameter change rate exceeds 100% in this manner, the dispersibility and dispersion stability of the obtained oxidized CNT in water can be further improved.
[0037] In the present invention, the "average diameter of CNTs" can be determined using the method described in Examples of the present specification.
[0038] Effects of the Invention
[0039] According to the present invention, it is possible to provide oxidized carbon nanotubes having excellent dispersibility and dispersion stability in water.
[0040] Furthermore, according to the present invention, it is possible to provide a method for producing oxidized carbon nanotubes having excellent dispersibility and dispersion stability in water. DETAILED DESCRIPTION
[0041] Hereinafter, embodiments of the present invention will be described in detail.
[0042] Here, the oxidized CNTs of the present invention are not particularly limited and can be used, for example, as electronic components such as electronic circuits like logic circuits, memories such as DRAM, SRAM, and NRAM, semiconductor devices, interconnects, complementary MOS, bipolar transistors, etc.; chemical sensors such as detectors for trace gases, etc.; biosensors such as detectors for DNA, proteins, etc.; and constituent elements of such electronic products in the manufacturing process of electronic products such as conductive films for solar cells, touch panels, etc. Moreover, the oxidized CNTs of the present invention can be efficiently manufactured by the manufacturing method of the oxidized CNTs of the present invention.
[0043] (Oxidized CNT)
[0044] The oxidized CNTs of the present invention need to contain oxidized single-walled CNTs in a specified ratio and have a D' band.
[0045] (Ratio of the number of oxidized single-walled CNTs to the total number of oxidized CNTs)
[0046] Moreover, for the oxidized CNTs of the present invention, the ratio of the number of oxidized single-walled CNTs to the total number of oxidized CNTs needs to be greater than 50%, more preferably greater than 60%, preferably less than 85%, more preferably less than 80%, and further preferably less than 70%. If the ratio of the number of oxidized single-walled CNTs to the total number of oxidized CNTs is greater than 50%, the properties such as conductivity, thermal conductivity, and strength of the oxidized single-walled CNTs can be inhibited from being damaged. On the other hand, if the ratio of the number of oxidized single-walled CNTs to the total number of oxidized CNTs is less than 85%, the dispersibility and dispersion stability of the oxidized CNTs in water are improved.
[0047] (D' band)
[0048] The D' band is a Raman spectrum observed by Raman spectroscopy around 1620 cm -1 . Since the oxidized CNTs of the present invention have a D' band, it is considered that the oxidized CNTs have multiple oxidized edge portions. Moreover, it is considered that due to the electrostatic repulsion caused by such edge portions acting between the oxidized CNTs and, in addition, by cutting the CNTs starting from the edge portions to shorten the CNTs, the oxidized CNTs of the present invention are difficult to aggregate and have excellent dispersibility and dispersion stability in water.
[0049] (Average diameter of the oxidized CNTs)
[0050] Here, the average diameter of the oxidized CNTs of the present invention is preferably 3.5 nm or more, more preferably 3.7 nm or more, preferably 5 nm or less, and more preferably 4 nm or less. If the average diameter of the oxidized CNTs is 3.5 nm or more and 5 nm or less, the electrostatic repulsion acting between the oxidized CNTs can be increased, and the dispersibility of the oxidized CNTs can be improved.
[0051] <Oxygen Atomic Ratio of Oxidized CNT>
[0052] In addition, the oxygen atomic ratio of the oxidized CNT of the present invention is preferably 15 at% or more, preferably 30 at% or less, and more preferably 20 at% or less. If the oxygen atomic ratio of the oxidized CNT is 15 at% or more, the dispersibility and dispersion stability of the oxidized CNT in water can be further improved. On the other hand, if the oxygen atomic ratio of the oxidized CNT is 30 at% or less, the electrical conductivity, thermal conductivity, strength and other characteristics of the CNT can be suppressed from being damaged.
[0053] <Average Length of Oxidized CNTs>
[0054] Furthermore, the average length of the oxidized CNTs of the present invention is preferably 30 nm or more, more preferably 400 nm or more, preferably 120 nm or less, and more preferably 90 nm or less. If the average length of the oxidized CNTs is 30 nm or more, it is possible to further suppress the loss of the electrical conductivity, thermal conductivity, strength and other characteristics of the CNTs. On the other hand, if the average length of the oxidized CNTs is 120 nm or less, it is possible to further improve the dispersibility of the oxidized CNTs in water.
[0055] <G / D Ratio of Oxidized CNT>
[0056] Furthermore, the G / D ratio of the oxidized CNT of the present invention is preferably greater than 0.6 and not more than 2, and more preferably not more than 1. When the G / D ratio of the oxidized CNT is greater than 0.6 and not more than 2, the oxidized CNT has better dispersibility in water.
[0057] <G / D' Ratio of Oxidized CNT>
[0058] The G / D' ratio of the oxidized CNT of the present invention is preferably 1.0 to 2.0, and more preferably 1.5 to 1.0. When the G / D' ratio of the oxidized CNT is 1.0 to 2.0, the oxidized CNT has better dispersibility in water.
[0059] In the present invention, the "G / D' ratio" refers to the ratio of the intensity of the D' band peak to the intensity of the G band peak in the Raman spectrum. The "G / D' ratio" can be determined using the method described in Examples of the present specification.
[0060] Furthermore, the above-mentioned method for producing oxidized CNTs can be efficiently produced by using the method for producing oxidized CNTs of the present invention described below.
[0061] (Method for producing oxidized CNT)
[0062] The manufacturing method of the oxidized CNT of the present invention needs to include an oxidation treatment step of oxidizing CNTs containing single-walled CNTs, and the BET specific surface area of the CNTs is greater than 1300 m 2 / g. It should be noted that the CNTs used in the manufacturing method of the present invention do not have a D' band in the Raman spectrum.
[0063] Moreover, according to the manufacturing method of the oxidized CNT of the present invention, an oxidized CNT excellent in dispersibility and dispersion stability in water can be manufactured. Although the reason is not clear yet, it is speculated as follows.
[0064] By oxidizing the CNTs, the surfaces of the CNTs are functionalized, and a plurality of oxidized edge portions are formed on the surfaces of the CNTs. At the same time, the CNTs are cut starting from these edge portions to form oxidized CNTs. It can be considered that if the manufacturing method of the present invention is used, through the interaction of the formation of the edge portions and the cutting of the CNTs based on such oxidation treatment, an oxidized CNT excellent in dispersibility and dispersion stability in water can be efficiently manufactured.
[0065] <BET specific surface area of CNTs>
[0066] The specific surface area of the CNTs used in the manufacturing method of the present invention needs to be greater than 1300 m 2 / g, preferably greater than 1400 m 2 / g. By using CNTs with a specific surface area greater than 1300 m 2 / g, the oxidation treatment can be efficiently carried out, and the manufacturing efficiency of the oxidized CNTs can be improved.
[0067] Moreover, from the viewpoint of improving the manufacturing efficiency of the oxidized CNTs, the CNTs used in the manufacturing method of the present invention more preferably have the following properties.
[0068] <Ratio of the number of single-walled CNTs to the total number of CNTs>
[0069] In the CNTs used in the manufacturing method of the present invention, the ratio of the number of single-walled CNTs to the total number of CNTs is preferably greater than 80%, and more preferably greater than 90%. If the ratio of the number of single-walled CNTs to the total number of CNTs is greater than 80%, the dispersibility and dispersion stability of the obtained oxidized CNTs in water are improved.
[0070] <Average diameter of CNTs>
[0071] In addition, the average diameter (Av) of the CNTs used in the manufacturing method of the present invention is preferably 2.0 nm or more, more preferably 2.5 nm or more, preferably 3.5 nm or less, and more preferably 3.0 nm or less. If the average diameter (Av) of the CNTs is 2.0 nm or more and 3.5 nm or less, oxidized CNTs with more excellent dispersibility and dispersion stability can be manufactured.
[0072] <Oxygen atom ratio of CNT>
[0073] Furthermore, the oxygen atom ratio of the CNTs used in the manufacturing method of the present invention is generally 2.0 at% or less, preferably 1.8 at% or less, and more preferably 1.5 at% or less.
[0074] <Average length of CNT>
[0075] Moreover, the average length of the CNTs used in the manufacturing method of the present invention is preferably 600 μm or less, more preferably 500 μm or less, and further preferably 400 μm or less when synthesizing the CNTs. If the length during the synthesis of the CNTs is 600 μm or less, oxidized CNTs can be manufactured more efficiently.
[0076] <G / D ratio of CNT>
[0077] In addition, the G / D ratio of the CNTs used in the manufacturing method of the present invention is preferably greater than 3.0, more preferably greater than 4.0, preferably less than 10, and more preferably 5.0 or less. If the G / D ratio of the CNTs is greater than 3.0 and less than 10, the obtained oxidized CNTs have more excellent dispersibility in water.
[0078] <Aspect ratio of CNT>
[0079] Furthermore, the aspect ratio (length / diameter) of the CNTs used in the manufacturing method of the present invention is preferably greater than 10. In addition, the aspect ratio of the CNTs can be obtained by measuring the diameters and lengths of 100 randomly selected CNTs using a transmission electron microscope and calculating the average value of the ratio of diameter to length (length / diameter).
[0080] <t-curve of CNT>
[0081] In addition, the CNTs used in the manufacturing method of the present invention preferably have a t-curve that is convex upward according to the adsorption isotherm. More preferably, the t-curve is convex upward without performing an opening treatment on the CNTs. If CNTs with a t-curve that is convex upward according to the adsorption isotherm are used, the dispersibility of the obtained oxidized CNTs in water can be further improved.
[0082] Here, adsorption generally refers to the phenomenon that gas molecules are removed from the gas phase and moved to the solid surface, and can be classified into physical adsorption and chemical adsorption according to the cause. In addition, physical adsorption is used in the nitrogen adsorption method for obtaining the t-curve. In addition, usually if the adsorption temperature is fixed, the greater the pressure, the greater the number of nitrogen molecules adsorbed on the CNT. In addition, a curve drawn with the horizontal axis as the relative pressure (the ratio of the pressure P in the adsorption equilibrium state to the saturated vapor pressure P0) and the vertical axis as the nitrogen adsorption amount is called an "isotherm", and the situation in which the nitrogen adsorption amount is measured while increasing the pressure is called an "adsorption isotherm", and the situation in which the nitrogen adsorption amount is measured while reducing the pressure is called a "desorption isotherm".
[0083] Furthermore, the t-curve can be obtained by converting the relative pressure into the average thickness t (nm) of the nitrogen adsorption layer in the adsorption isotherm measured by the nitrogen adsorption method. That is, the average thickness t of the nitrogen adsorption layer corresponding to the relative pressure is obtained based on a known standard isotherm plotted with respect to the relative pressure P / P0, and the above conversion is performed to obtain the t-curve of CNT (t-curve method proposed by de Boer et al.).
[0084] Here, in the sample having fine pores on the surface, the growth of the nitrogen adsorption layer is divided into the following processes (1) to (3). Then, according to the following processes (1) to (3), the slope of the t-curve changes.
[0085] (1) The process of forming a monomolecular adsorption layer of nitrogen molecules on the entire surface;
[0086] (2) The formation of a multi-molecular adsorption layer and the accompanying capillary condensation filling process in the pores;
[0087] (3) The process of forming a multi-molecule adsorption layer on the seemingly non-porous surface whose pores are filled with nitrogen
[0088] Moreover, the t-curve, which is convex upward, is located on a straight line passing through the origin in a region where the average thickness t of the nitrogen adsorption layer is small, whereas when t increases, the curve is located at a position deviated downward from the straight line. CNTs having this t-curve shape indicate that the ratio of the internal specific surface area of the CNT to the total specific surface area is large, and that a large number of pores are formed in the CNT, resulting in the CNT being difficult to aggregate.
[0089] In addition, the inflection point of the t-curve of CNT is preferably in the range of 0.2≤t(nm)≤1.5, more preferably in the range of 0.45≤t(nm)≤1.5, and further preferably in the range of 0.55≤t(nm)≤1.0. When the position of the inflection point of the t-curve is within the above range, the characteristics of CNT are further improved, so the dispersibility of the obtained oxidized CNT in water can be further improved.
[0090] Here, the “position of the bending point” refers to the intersection of the approximate straight line A of the above-mentioned process (1) and the approximate straight line B of the above-mentioned process (3) in the t-curve.
[0091] Furthermore, the ratio (S2 / S1) of the internal specific surface area S2 to the total specific surface area S1 of the CNT used in the production method of the present invention obtained by the t-curve is preferably 0.05 or more, more preferably 0.06 or more, further preferably 0.08 or more, and preferably 0.30 or less. If S2 / S1 is 0.05 or more and 0.30 or less, the characteristics of the CNT can be further improved, and thus the dispersibility of the obtained oxidized CNT in water can be further improved.
[0092] In addition, the measurement of the adsorption isotherm of CNTs, the preparation of t-curves, and the calculation of the total specific surface area S1 and the internal specific surface area S2 based on the analysis of the t-curve can be performed using, for example, a commercially available measuring device "BELSORP (registered trademark)-mini" (manufactured by BEL Corporation of Japan).
[0093] [3σ / Av of CNT]
[0094] Here, as CNTs used in the production method of the present invention, it is preferred to use CNTs having a ratio (3σ / Av) of the value (3σ) multiplied by 3 of the standard deviation (σ) of the diameter to the average diameter (Av) of greater than 0.20 and less than 0.80, more preferably CNTs having 3σ / Av greater than 0.25, further preferably CNTs having 3σ / Av greater than 0.40, and particularly preferably CNTs having 3σ / Av greater than 0.50. If CNTs having 3σ / Av greater than 0.20 and less than 0.80 are used, the dispersibility of the obtained oxidized CNTs in water can be further improved.
[0095] In addition, the "average diameter (Av) of CNTs" and the "standard deviation of the diameter of CNTs (σ: sample standard deviation)" can be obtained by measuring the diameters (outer diameters) of 100 randomly selected CNTs using a transmission electron microscope. Moreover, the average diameter (Av) and standard deviation (σ) of CNTs can be adjusted by changing the synthesis method and synthesis conditions of CNTs, or by combining a plurality of CNTs obtained by different synthesis methods.
[0096] [CNT synthesis method]
[0097] The synthesis method of CNTs used in the manufacturing method of the present invention is not particularly limited. Moreover, CNTs having the above properties can be efficiently synthesized, for example, by forming a catalyst layer on the surface of a substrate using a wet process in the following method. The method is to supply a raw material compound and a carrier gas to a substrate having a catalyst layer for CNT synthesis on its surface, and when synthesizing CNTs by chemical vapor deposition (CVD method), a trace amount of an oxidizing agent (catalyst activating substance) is present in the system, thereby significantly improving the catalytic activity of the catalyst layer (super growth method; refer to International Publication No. 2006 / 011655).
[0098] Moreover, from the viewpoint of efficiently synthesizing CNTs with a large specific surface area, it is preferable to synthesize CNTs by the following method: that is, a method of repeatedly synthesizing CNTs by CVD method using a substrate on which a catalyst layer used in the synthesis of CNTs is formed (for example, refer to Japanese Patent Laid-Open No. 2015-188811). Moreover, this preferred method for synthesizing CNTs can include, for example, the following steps: a CNT peeling step of peeling CNTs from a substrate on which CNTs are formed; a step of manufacturing a reused substrate using the used substrate from which CNTs are peeled from the substrate in the CNT peeling step (reused substrate manufacturing step); a step of manufacturing a catalyst substrate for CNT growth using the obtained reused substrate (catalyst substrate manufacturing step); and a CNT growth step of synthesizing CNTs on the catalyst substrate for CNT growth by CVD method using the obtained catalyst substrate for CNT growth. Hereinafter, each step will be described in turn.
[0099] <CNT Peeling Step>
[0100] In the CNT peeling step, CNTs are peeled from a substrate having CNTs formed on its surface, and a used substrate from which CNTs have been peeled from the surface is obtained.
[0101] Here, as a method for peeling CNTs from a substrate in the CNT peeling step, physical, chemical, or mechanical peeling methods can be cited. Specifically, for example, a method of peeling using an electric field, a magnetic field, a centrifugal force, a surface tension, etc.; a method of mechanically directly peeling and removing from the substrate; and a method of peeling from the substrate using pressure or heat, etc. can be applied. In addition, CNTs can also be sucked by a vacuum pump and peeled and removed from the substrate. Further, as a simple and less-damaging peeling method, a method of directly picking up CNTs from the substrate with tweezers can be cited; a method of peeling CNTs from the substrate using a thin tool such as a plastic scraper or a cutting blade having a sharp part. As the peeling method, a method of peeling CNTs from the substrate using a thin tool such as a plastic scraper or a cutting blade having a sharp part is particularly preferred.
[0102] <Reused Substrate Manufacturing Step>
[0103] The reused substrate production step includes an initialization step of washing the used substrate obtained in the CNT exfoliation step, and optionally includes a cleaning step of cleaning the used substrate that has undergone the initialization step.
[0104] [Used substrate]
[0105] As a used substrate, for example, a used substrate obtained by stripping CNT from a substrate on which CNT synthesis has been performed only once can be used. The used substrate may also have, for example, a substrate, a base layer on the substrate, and a catalyst layer on the base layer. Moreover, impurities such as carbon components attached when synthesizing CNTs or carbon components remaining when stripping CNTs remain on the surface of at least the catalyst layer side of the used substrate (i.e., the surface on which the CNT side is formed). Specifically, it is speculated that carbon compounds such as CNTs, graphite-like or amorphous nanoparticles, and flaky substances that are not cut off and remain when stripping CNTs remain on the surface of the used substrate. In addition, the structure of the used substrate other than impurities, i.e., the substrate, the base layer, and the catalyst layer are substances used when synthesizing CNTs stripped from the substrate in the CNT stripping process. Therefore, for example, the catalyst layer is composed of a particulate CNT synthesis catalyst that is not stripped and remains when stripping CNTs.
[0106] -Base Material-
[0107] Here, as a substrate constituting a part of the used substrate after being used in the synthesis of CNT, any substrate can be used as long as it can carry a catalyst for CNT synthesis on its surface and has resistance to cleaning by collision of liquid described later. Specifically, as a substrate, a substrate having a practical effect in the synthesis of CNT can be appropriately used. In addition, the substrate is preferably able to maintain its shape even at a high temperature of 50°C or above.
[0108] Here, as the material of the substrate, metals such as iron, nickel, chromium, molybdenum, tungsten, titanium, aluminum, manganese, cobalt, copper, silver, gold, platinum, niobium, tantalum, lead, zinc, gallium, indium, germanium and antimony, and alloys and oxides containing these metals, or non-metals such as silicon, quartz, glass, mica, graphite and diamond, and ceramics, etc. Among these, metals are low in cost and easy to process compared with silicon and ceramics, so they are preferred, and Fe-Cr (iron-chromium) alloys, Fe-Ni (iron-nickel) alloys, Fe-Cr-Ni (iron-chromium-nickel) alloys, etc. are particularly preferred.
[0109] Examples of the shape of the substrate include a flat plate, a film, a bulk, or a granular shape. From the viewpoint of synthesizing a large amount of CNTs, a flat plate and a granular shape are particularly advantageous.
[0110] - Basal layer -
[0111] The base layer is also called a "catalyst supporting layer" and is a layer that becomes the base of the CNT synthesis catalyst. Moreover, as the material of the base layer, various materials can be used as long as they are materials that become the base of the CNT synthesis catalyst, preferably ceramic materials such as aluminum oxide, titanium oxide, titanium nitride, silicon oxide, etc. As the material of the base layer, ceramic materials are particularly preferably used. This is because ceramic materials make CNT grow better when the substrate is reused to synthesize CNT.
[0112] Furthermore, from the viewpoint of stabilizing the growth of CNTs and improving the yield, the thickness of the base layer is preferably 10 nm or more, and from the viewpoint of production efficiency, it is preferably 50 nm or less.
[0113] - Catalyst layer -
[0114] The catalyst layer is a layer of particles containing a CNT synthesis catalyst. Here, as the CNT synthesis catalyst constituting the catalyst layer, for example, a catalyst that has been practically effective in the synthesis of CNTs to date can be appropriately used. Specifically, as the CNT synthesis catalyst, iron, nickel, cobalt, molybdenum, and chlorides and alloys thereof can be cited.
[0115] In addition, the amount of the CNT synthesis catalyst used to form the catalyst layer can be, for example, an amount that has been practically effective in the synthesis of CNTs to date. Specifically, for example, when iron is used as the CNT synthesis catalyst, the thickness of the catalyst layer is preferably 0.1 nm to 100 nm, more preferably 0.5 nm to 5 nm, and particularly preferably 0.8 nm to 2 nm.
[0116] Here, examples of the combination of the base layer and the catalyst layer include an aluminum oxide-iron thin film, an aluminum oxide-cobalt thin film, and an aluminum oxide-iron-molybdenum thin film.
[0117] [Initialization process]
[0118] In the initialization process, the used substrate from which the CNTs have been stripped is cleaned by the collision of a liquid. Specifically, in the initialization process, at least the surface of the side from which the CNTs have been stripped of the used substrate is cleaned by the collision of a liquid. In the initialization process, by cleaning by the collision of a liquid, impurities such as carbon components remaining on the surface of the used substrate can be removed.
[0119] In addition, the base layer and the catalyst layer may remain on the substrate after the initialization process, and the base layer and the catalyst layer of the used substrate may also be removed as the carbon component is removed by the collision of the liquid. In addition, even if the base layer and the catalyst layer are removed in the initialization process, if the base layer and the catalyst layer are formed again in the base layer forming process and the catalyst forming process described later, it will not have an adverse effect on the subsequent generation of CNTs. On the other hand, when the carbon component is not fully removed in the initialization process, even if the base layer and the catalyst layer are formed thereon, the production and quality of CNTs will decrease in the subsequent generation of CNTs.
[0120] Here, "cleaning by collision of liquid" refers to the following method: making liquid collide with the surface of a used substrate as the object to be cleaned, and utilizing the local high pressure field, shear flow, vibration of the object to be cleaned, etc. generated when the liquid is collided, to physically clean the surface of the used substrate.
[0121] Furthermore, as a method of cleaning utilizing collision of liquid, for example, ultrasonic cleaning can be cited.
[0122] -Ultrasonic cleaning-
[0123] Here, when the used substrate is cleaned by ultrasonic cleaning, for example, the used substrate is immersed in a liquid such as water, and ultrasonic waves are irradiated to cause the liquid to collide with the used substrate while vibrating. Then, the surface of the used substrate is cleaned by utilizing cavitation, shear flow, vibration of the used substrate, etc. generated by the irradiation of ultrasonic waves.
[0124] In addition, for ultrasonic cleaning, a known ultrasonic cleaning device such as an ultrasonic cleaning tank can be used.
[0125] Moreover, the ultrasonic cleaning of the used substrate is preferably carried out at a frequency of more than 20kHz and less than 5MHz, more preferably at a frequency of more than 20kHz and less than 1MHz, and further preferably at a frequency of more than 20kHz and less than 200kHz. Cavitation can be moderately generated in this frequency band, and cleaning can be performed efficiently. In addition, the time for ultrasonic cleaning is preferably more than 0.1 minutes and less than 10 minutes. Furthermore, the temperature during ultrasonic cleaning is preferably more than 20°C and less than 50°C. This is because when the frequency is too high, or the cleaning time is too long, or the temperature is too high, the substrate used in cleaning may deteriorate. On the other hand, it is also because when the frequency is too low, or the cleaning time is too short, or the temperature is too low, impurities such as carbon components may not be fully removed.
[0126] [Cleaning process]
[0127] In the cleaning process, the substrate after the initialization process is cleaned to obtain a reused substrate in which impurities such as carbon components are removed from the used substrate. In the cleaning process, the substrate is cleaned using a method different from the cleaning method used in the initialization process, such as a method of washing the substrate surface with water and wiping it with a cloth, a method of washing the substrate surface with water and spraying air to dry it, etc. Although sometimes impurities such as carbon components are not completely removed and remain on the surface of the substrate after cleaning by the collision of liquid, by cleaning the substrate after the initialization process, the remaining impurities such as carbon components can be fully removed. In addition, the adhesion between the carbon components and the substrate remaining on the surface of the substrate is reduced by cleaning by the collision of liquid in the initialization process. Therefore, in the cleaning process, the carbon components and the like can be easily removed by washing with water, wiping, etc.
[0128] Here, the base layer and the catalyst layer may remain on the substrate after the cleaning process, and the base layer and the catalyst layer may also be removed as the surface of the substrate is cleaned. In addition, even if the base layer and the catalyst layer are removed in the cleaning process, if the base layer and the catalyst layer are formed in the base layer forming process and the catalyst forming process described later, it will not have an adverse effect on the subsequent generation of CNTs.
[0129] [Recycling base material]
[0130] Furthermore, the reused base material obtained by subjecting the used base material to the initialization step and the optional cleaning step in the above-mentioned reused base material production step has a structure in which impurities such as carbon components are removed from the used base material.
[0131] Here, the surface of the reused substrate has had carbon components and the like removed in the aforementioned initialization process and cleaning process. Therefore, after the reused substrate is formed into a base layer and a catalyst layer in the catalyst substrate manufacturing process described in detail later to be made into a catalyst substrate for CNT growth, it can be used again for CNT synthesis. That is, the reused substrate can be used as a raw material substrate when manufacturing a catalyst substrate for CNT growth in the catalyst substrate manufacturing process described in detail later.
[0132] In addition, when the recycled substrate is reused for synthesizing CNTs, if the recycled substrate contains impurities such as carbon components, the growth of CNTs may be unstable or the quality of the generated CNTs may be reduced. However, when manufacturing the recycled substrate, since the carbon components are fully removed in the aforementioned initialization process and cleaning process, if the recycled substrate is used, the growth of CNTs can be stabilized and high-quality CNTs can be repeatedly generated.
[0133] Here, as a method for removing the carbon components attached to the substrate, a method of evaporating or ashing by high temperature heating, a method of pickling, etc. can be considered. However, when the substrate is heated at a high temperature, problems such as damage to the substrate and warping of the substrate may occur, which may sometimes have an adverse effect on the growth of CNTs when reused. In addition, when the substrate is pickled, especially when the substrate is made of a metal material, the substrate will be corroded, which may have an adverse effect on the growth of CNTs when reused.
[0134] In contrast, since the carbon components are removed by the collision of liquids such as water during the initialization process, the degradation of the substrate during cleaning (such as damage, warping, and corrosion) can be suppressed. Therefore, if a reused substrate is used, the growth of CNTs can be stabilized and high-quality CNTs can be repeatedly generated.
[0135] -Properties of recycled substrates-
[0136] Here, as described above, it is preferred that carbon components are sufficiently removed from the recycled substrate, and it is particularly preferred that no carbon components remain on the surface of the recycled substrate. Here, the removal of carbon components from the recycled substrate can be evaluated by, for example, Raman spectroscopy of the substrate surface. In the Raman spectrum, carbon components can be detected as 1593 cm -1 Vibrational modes of graphite near 1350cm -1 Therefore, it is preferable that these peaks are not observed by reusing the substrate.
[0137] In addition, the contact angle between the surface of the recycled substrate (the surface on the catalyst layer side) and water is preferably 70° or less, and more preferably 65° or less. If the contact angle of the surface of the recycled substrate is large, it may have an adverse effect on the growth of CNTs when it is used again to synthesize CNTs.
[0138] The contact angle can be calculated by dropping 2 microliters of pure water onto the surface of the reused substrate on the catalyst layer side and using the θ / 2 method from the droplet after 5 seconds.
[0139] <Catalyst substrate manufacturing process>
[0140] The catalyst substrate manufacturing step includes at least a catalyst layer forming step, in which a catalyst for CNT synthesis is supported on the surface of the reused substrate obtained in the reused substrate manufacturing step to form a catalyst layer on the reused substrate. In addition, the catalyst substrate manufacturing step may also arbitrarily include a base layer forming step before the catalyst layer forming step, in which a base layer serving as a base of the CNT synthesis catalyst is formed on the surface of the reused substrate.
[0141] Here, when a recycled substrate is used to synthesize CNTs, it is possible to directly use the recycled substrate with the catalyst layer located on the outermost surface for the second CNT synthesis. However, when the recycled substrate is directly used, sometimes the growth of CNTs becomes unstable or the quality of the generated CNTs decreases. Possible reasons include: the density and diameter of the catalyst particles in the catalyst layer are different from those in the first CNT synthesis; the catalyst particles in the catalyst layer are removed in the initialization process and the cleaning process, etc.
[0142] Therefore, in the catalyst substrate manufacturing process, the CNT synthesis catalyst is loaded again on the surface of the reused substrate, and the catalyst layer is formed again on the reused substrate. In addition, if a base layer is formed on the reused substrate before the catalyst layer is formed again, the used catalyst layer can be separated from the catalyst layer for the next CNT synthesis by the base layer, and the catalyst layer can be well formed. Therefore, in the catalyst substrate manufacturing process, it is preferred to implement a base layer forming process.
[0143] [Base layer forming step]
[0144] The base layer may be formed on the catalyst layer of the reused substrate by a wet process or a dry process (sputtering evaporation method, etc.) The wet process is preferably used from the viewpoints of simplicity of the film forming apparatus, throughput speed, and low cost of raw materials.
[0145] Hereinafter, a case where the base layer is formed by a wet process will be described as an example.
[0146] The wet process for forming the base layer comprises the steps of dissolving a metal organic compound and / or a metal salt containing an element to form the base layer in an organic solvent to form a coating liquid A, applying the coating liquid A on the substrate, and then heating the substrate.
[0147] Here, for example, when an aluminum oxide film is used as a base layer, aluminum alkoxides such as aluminum trimethoxide, aluminum triethoxide, aluminum tri-n-propoxide, aluminum triisopropoxide, aluminum tri-n-butoxide, aluminum tri-sec-butoxide, and aluminum tri-tert-butoxide can be used as metal organic compounds and / or metal salts for forming the aluminum oxide film. Coordination compounds such as tri(acetylacetonate)aluminum (III) can also be mentioned as metal organic compounds for forming the aluminum oxide film. As metal salts, aluminum sulfate, aluminum chloride, aluminum nitrate, aluminum bromide, aluminum iodide, aluminum lactate, basic aluminum chloride, and basic aluminum nitrate can be mentioned. Among these, aluminum alkoxides are particularly preferably used. These can be used alone or in the form of a mixture of two or more.
[0148] As the organic solvent, various organic solvents such as alcohols, glycols, ketones, ethers, esters, hydrocarbons, etc. can be used, but from the aspect of good solubility of metal organic compounds and metal salts, alcohols or glycols are preferably used. These organic solvents can be used alone or in combination of two or more. As alcohol, methanol, ethanol, 2-propanol (isopropanol) etc. are preferred from the aspect of handleability and storage stability.
[0149] As a coating method of the coating liquid A, any method such as a coating method by spraying, brushing, etc., spin coating, dip coating, etc. can be used, but dip coating is preferred from the viewpoint of productivity and film thickness control.
[0150] After coating the coating liquid A, heating can be performed for 5 minutes to 3 hours at a temperature range of 50°C to 400°C, depending on the type of the base layer. By heating, the coated metal organic compound and / or metal salt begins to hydrolyze and undergo polycondensation reaction, forming a cured film (base layer) containing metal hydroxide and / or metal oxide on the surface of the recycled substrate.
[0151] [Catalyst layer forming step]
[0152] The catalyst layer can be formed by either a wet process or a dry process (sputtering evaporation method, etc.) as with the base layer. The wet process is preferably used from the viewpoints of simplicity of the film forming apparatus, throughput speed, and low cost of raw materials.
[0153] Hereinafter, a case where the catalyst layer is formed by a wet process will be described as an example.
[0154] The wet process for forming the catalyst layer comprises the steps of dissolving a metal organic compound and / or a metal salt containing an element to be a CNT synthesis catalyst in an organic solvent to form a coating liquid B, applying the coating liquid B on a substrate, and then heating the substrate.
[0155] Here, for example, when iron is used as a catalyst for CNT synthesis, as a metal organic compound and / or metal salt for forming an iron film that becomes a catalyst layer, pentacarbonyl iron, ferrocene, acetylacetonate iron (II), acetylacetonate iron (III), trifluoroacetylacetonate iron (II), trifluoroacetylacetonate iron (III), etc. can be used. As metal salts, inorganic acid irons such as ferric sulfate, ferric nitrate, ferric phosphate, ferric chloride, ferric bromide, organic acid irons such as ferric acetate, ferric oxalate, ferric citrate, and ferric lactate can be cited. Among these, organic acid iron is preferably used. These can be used alone or in the form of a mixture of two or more.
[0156] In addition, as the organic solvent of Coating Liquid B, the same organic solvents as those of the above-mentioned Coating Liquid A can be used. Moreover, their contents can also be set to the same amounts as those of Coating Liquid A.
[0157] Furthermore, as the coating method of Coating Liquid B, the same method as that of Coating Liquid A can be used. In addition, the heating after Coating Liquid B is coated can also be carried out in the same manner as that of Coating Liquid A.
[0158] Through this catalyst layer formation process, a CNT growth catalyst substrate with a catalyst layer formed on the surface of the recycled substrate is formed.
[0159] [CNT growth catalyst substrate]
[0160] Moreover, the CNT growth catalyst substrate obtained by performing the base layer formation process and the catalyst layer formation process on the recycled substrate in the above-mentioned catalyst substrate manufacturing process has a structure in which a new base layer and a catalyst layer are sequentially laminated on the catalyst layer side of the recycled substrate, for example.
[0161] Since the base layer and the catalyst layer are newly formed on the recycled substrate, this CNT growth catalyst substrate can be preferably used when synthesizing CNTs in the CNT growth process described in detail below.
[0162] [CNT growth process]
[0163] In the CNT growth process, the CNT growth catalyst substrate obtained in the catalyst substrate manufacturing process is used, and CNTs are synthesized on the CNT growth catalyst substrate by a known method such as the CVD method. In addition, in the CNT growth process, since the CNT growth catalyst substrate with a newly formed base layer and catalyst layer on the recycled substrate is used, high-quality CNTs can be stably synthesized.
[0164] Specifically, in the CNT growth process, without particular limitation, a formation process of reducing the CNT synthesis catalyst on the CNT growth catalyst substrate and a growth process of growing CNTs are carried out, and CNTs can be grown on the CNT growth catalyst substrate.
[0165] [CNT production device]
[0166] In addition, the CNT growth process is not particularly limited, and can be implemented using a known CNT production device having a synthesis furnace (reaction chamber) and a heating unit for accommodating a CNT growth catalyst substrate. Specifically, it is possible to use a known CNT production device such as a thermal CVD furnace, a thermal heating furnace, an electric furnace, a drying furnace, a constant temperature bath, an atmosphere furnace, a gas replacement furnace, a muffle furnace, an oven, a vacuum heating furnace, a plasma reaction furnace, a microplasma reaction furnace, an RF plasma reaction furnace, an electromagnetic wave heating reaction furnace, a microwave irradiation reaction furnace, an infrared irradiation heating furnace, an ultraviolet heating reaction furnace, an MBE reaction furnace, an MOCVD reaction furnace, a laser heating device, etc.
[0167] Then, in the CNT growth step, CNTs are synthesized on the CNT growth catalyst substrate, and CNTs are formed on the CNT growth catalyst substrate.
[0168] <Oxidation treatment>
[0169] Then, in the oxidation treatment step of the manufacturing method of the present invention, the CNTs containing single-walled CNTs are subjected to oxidation treatment. Here, the oxidation treatment method is not particularly limited, and can be carried out by, for example, contacting the CNTs with an acidic solution below pH 2 (acid treatment). Moreover, the method for contacting the acid with the CNTs is not particularly limited, and can be carried out by, for example, adding CNTs to an acidic solution below pH 2 to obtain a mixed solution, and oxidizing the CNTs. At this time, as an acidic solution, it is not particularly limited, and for example, nitric acid, hydrochloric acid, sulfuric acid, and mixed acid can be used. These can be used alone or in combination of two or more. From the viewpoint of further improving the dispersibility of the oxidized CNTs in water, it is particularly preferred to use nitric acid.
[0170] Here, as a mixing method for obtaining a mixed solution, any method can be used for stirring. In addition, the stirring time when the mixed solution is obtained is preferably 0.1 hours or more and 10 hours or less. Furthermore, the reflux temperature when the mixed solution is refluxed is preferably 100°C or more and 150°C or less, and the reflux time is preferably 3 hours or more and 20 hours or less. If the reflux temperature and the reflux time are within the above ranges, respectively, the oxidation treatment can be fully carried out, further improving the dispersibility and dispersion stability of the obtained oxidized CNT in water.
[0171] Here, as the solvent of the acidic solution, there is no particular limitation, and water, any organic solvent (such as esters, ketones, alcohols) can be used. These solvents can be used alone or in combination of two or more. Moreover, water is preferred among these. Moreover, from the viewpoint of improving the manufacturing efficiency of oxidized CNTs, it is preferred to use an aqueous nitric acid solution with a concentration greater than 40% by mass, more preferably greater than 50% by mass, and further preferably greater than 60% by mass as the acidic solution for oxidation treatment. If this is done, the CNTs are cut shorter by increasing the number of edge portions generated on the surface of the CNTs, thereby being able to improve the dispersibility and dispersion stability of the obtained oxidized CNTs.
[0172] Furthermore, in the production method of the present invention, it is preferred that in the oxidation treatment step, the mixture containing CNTs and the nitric acid aqueous solution is refluxed at a temperature of ±5° C. or higher than the azeotropic point of the nitric acid aqueous solution. In this way, the oxidation treatment can be sufficiently performed, and the production efficiency of oxidized CNTs can be further improved.
[0173] [Single wall ratio change rate]
[0174] Furthermore, in the production method of the present invention, in the oxidation treatment step, the CNT is preferably oxidized so that the single-wall ratio change rate represented by the following formula (1) becomes 90% or less.
[0175] Single wall ratio change rate = SGCNT A / SGCNT B ×100(%)…Formula (1)
[0176] In formula (1), SGCNT A The ratio of the number of oxidized single-walled CNTs to the total number of oxidized CNTs is represented by SGCNT. B Indicates the ratio of the number of single-walled CNTs to the total number of CNTs. By performing the oxidation treatment so that the change rate of the single-wall ratio is 90% or less, the dispersibility and dispersion stability of the obtained oxidized CNTs in water can be further improved.
[0177] [Average diameter change rate]
[0178] Furthermore, in the production method of the present invention, in the oxidation treatment step, the carbon nanotubes are preferably oxidized so that the average diameter change rate represented by the following formula (2) is greater than 100%.
[0179] Average diameter change rate = CNT DA / CNT DB ×100(%)…Formula (2) In formula (2), CNT DA represents the average diameter of oxidized carbon nanotubes, CNT DBRepresents the average diameter of the carbon nanotubes. In this way, by performing the oxidation treatment at an average diameter change rate of more than 100%, the dispersibility and dispersion stability of the obtained oxidized CNTs in water can be further improved.
[0180] Moreover, the oxidized CNTs obtained by the production method of the present invention can be dispersed in water and used in the form of an oxidized CNT aqueous dispersion, for example. At this time, the concentration of the oxidized CNTs in the oxidized CNT aqueous dispersion is not particularly limited and can be adjusted as appropriate.
[0181] Examples
[0182] Hereinafter, the present invention will be specifically described based on examples, but the present invention is not limited to these examples.
[0183] Moreover, in the examples and comparative examples, the BET specific surface area, G / D ratio, D' band, G / D' ratio, the proportion of the number of single-walled CNTs in the total number of CNTs, the proportion of the number of oxidized single-walled CNTs in the total number of oxidized CNTs, the average diameter of CNTs and oxidized CNTs, the oxygen atom ratio of CNTs and oxidized CNTs, the average length of CNTs and oxidized CNTs, the single-walled ratio change rate, the average diameter change rate, the absorbance ratio, and the dispersion stability were measured and evaluated by the following methods, respectively.
[0184] <BET specific surface area>
[0185] According to JIS Z8830, using a BET specific surface area measuring device (manufactured by Mountech Co., Ltd., HM model-1210), the BET specific surface area (m 2 / g) of the CNTs was measured.
[0186] <G / D ratio>
[0187] Using a microscopic laser Raman spectrometer (Nicolet Almega XR manufactured by Thermo Fisher Scientific Inc.), the Raman spectra of CNTs and oxidized CNTs were measured respectively.
[0188] Then, for the obtained Raman spectra, the intensity of the G band peak observed near 1590 cm -1 and the intensity of the D band peak observed near 1340 cm -1 were obtained, and the G / D ratio was calculated.
[0189] <D' band, G / D' ratio>
[0190] By comparing the G band observed near 1590 cm -1 in the Raman spectrum of the oxidized CNTs and the G band observed near 1620 cm -1The D' band observed nearby is separated into two Gaussian function spectra to determine whether or not there is a D' band of oxidized CNT. This is specifically carried out in the following steps.
[0191] The Raman spectrum is as follows [Figure 1],
[0192] [Number 1]
[0193] Sp(v),
[0194] In the wave number region near the G band, that is, the region [number 2] below,
[0195] [Number 2]
[0196] 1500cm -1 ≤v≤1630cm -1
[0197] The G peak and D' peak are approximated using the Gaussian function of the following formula (a),
[0198] [Number 3]
[0199]
[0200]
[0201] Their sum, i.e. the following [Equation 4], is the original spectral function.
[0202] [Number 4]
[0203] Sp(v)≈G(v)+D′(v).
[0204] To reproduce the following [number 5],
[0205] [Number 5]
[0206] Sp(v),
[0207] The following [Equation 6] in the above equation (a) was optimized using the least squares method.
[0208] [Number 6]
[0209] g, d′, k, k′, v0, v′0.
[0210] The case where the calculation results converged and the peak separation was possible was defined as the presence of the D' band, and the case where the calculation results did not converge was defined as the absence of the D' band. The G / D' ratio was calculated from the calculated parameters. In addition, the meanings of the parameters shown in the above formula (a) are shown in Table 1 below.
[0211] [Table 1]
[0212] parameter meaning g The peak intensity of the G band d′ The peak intensity of the D′ band <![CDATA[v0]]> The peak wave number of the G band <![CDATA[v′0]]> Peak wave number of D′ band G / D′ Calculated by g / d′
[0213] <Ratio of the number of single-walled CNTs to the total number of CNTs, and ratio of the number of oxidized single-walled CNTs to the total number of oxidized CNTs>
[0214] The CNTs and oxidized CNTs were observed using a transmission electron microscope (TEM). From the obtained TEM images, the number of layers of 50 CNTs and 50 oxidized CNTs was measured. Then, the ratio of the number of single-walled CNTs to the 50 CNTs was taken as the "ratio of the number of single-walled CNTs to the total number of CNTs (SGCNT B )". In addition, the ratio of the number of oxidized single-walled CNTs to the 50 oxidized CNTs was taken as the "ratio of the number of oxidized single-walled CNTs to the total number of oxidized CNTs (SGCNT A )".
[0215] <Average diameter of CNTs and oxidized CNTs>
[0216] The CNTs and oxidized CNTs were observed using a transmission electron microscope (TEM). From the obtained TEM images, the diameters (outer diameters) of 50 CNTs and 50 oxidized CNTs were measured. Then, the arithmetic mean of the measured diameters of the CNTs and oxidized CNTs was taken as the average diameter of the CNTs (CNT DB ) and the average diameter of the oxidized CNTs (CNT DA ).
[0217] <Oxygen atom ratio of CNTs and oxidized CNTs>
[0218] The CNTs and oxidized CNTs were analyzed using an X-ray photoelectron spectroscopy apparatus (manufactured by Thermo Fisher Scientific Inc., VGTheta Probe). Then, the peak area of O1s and the total detected peak area were determined for the CNTs and oxidized CNTs, respectively. Based on these, the ratio (at%) of the amount of oxygen atoms (O) present to the total atomic weight of the surface atoms was calculated for the CNTs and oxidized CNTs respectively (=amount of O atoms present / total atomic weight×100), and the obtained value was taken as the oxygen atom ratio (at%).
[0219] <Average length of CNTs and oxidized CNTs>
[0220] The CNTs and oxidized CNTs were observed using a scanning electron microscope (SEM). From the obtained SEM images, the lengths of 50 CNTs and 50 oxidized CNTs were measured. Then, the arithmetic mean of the measured lengths of the CNTs and oxidized CNTs was taken as the average lengths of the CNTs and oxidized CNTs, respectively.
[0221] [Rate of change of single-wall ratio]
[0222] The proportion of single-walled CNTs in the total number of CNTs (SGCVT B ), the proportion of oxidized single-walled CNTs in the total number of oxidized CNTs (SGCVT A ), and the single-wall ratio change rate was calculated based on the following formula.
[0223] Single wall ratio change rate = SGCNT A / SGCNT B ×100(%)
[0224] [Average diameter change rate]
[0225] The average diameter of CNTs (CNT DB ), the average diameter of oxidized CNTs (CNT DA ), and the average diameter change rate was calculated based on the following formula.
[0226] Average diameter change rate = CNT DA / CNT DB ×100(%)
[0227] <Absorbance Ratio>
[0228] The oxidized CNT dispersion prepared in the examples and comparative examples was filtered and purified using a 0.2 μm syringe filter (manufactured by Pall Corporation, product name "Acrodisk Syringe Filter") to obtain a purified dispersion. Using the untreated oxidized CNT dispersion (unpurified dispersion) and the purified dispersion prepared in the examples and comparative examples, the absorbance at a path length of 1 mm and a wavelength of 550 nm was measured by a spectrophotometer (manufactured by JASCO Corporation, product name "V670"), respectively. Then, the absorbance ratio was calculated by the following formula. The larger the absorbance ratio, the higher the dispersibility of the oxidized CNT in water.
[0229] Absorbance ratio = (absorbance of purified dispersion) / (absorbance of unpurified dispersion)
[0230] <Dispersion stability>
[0231] The oxidized CNT dispersions prepared in the examples and comparative examples were stored at room temperature in a dark place for 1 month. The absorbance ratio of the oxidized CNT dispersions after storage was calculated. If the decrease in the absorbance ratio before and after storage was less than 0.1, the dispersion stability was judged to be "good", and if it was greater than 0.1, the dispersion stability was judged to be "poor".
[0232] (Example 1)
[0233] <Preparation of used substrate>
[0234] A coating liquid A was prepared by dissolving aluminum tri-sec-butoxide as an aluminum compound in 2-propanol.
[0235] Furthermore, coating liquid B was prepared by dissolving ferric acetate as an iron compound in 2-propanol.
[0236] The coating liquid A was applied to the surface of the Fe-Cr alloy SUS430 substrate as the substrate by dip coating at room temperature of 25°C and relative humidity of 50%. Specifically, the substrate was immersed in the coating liquid A, kept for 20 seconds, and the substrate was lifted at a lifting speed of 10 mm / sec. Then, it was air-dried for 5 minutes, heated in an air environment of 300°C for 30 minutes, and cooled to room temperature, thereby forming an aluminum oxide thin film (underlayer) with a film thickness of 40 nm on the substrate.
[0237] Next, the above-mentioned coating liquid B was applied to the aluminum oxide thin film provided on the substrate by dip coating at room temperature of 25°C and relative humidity of 50%. Specifically, the substrate with the aluminum oxide thin film was immersed in the coating liquid B, kept for 20 seconds, and then lifted up at a lifting speed of 3 mm / second. Then, it was air-dried for 5 minutes (drying temperature of 45°C), thereby forming an iron thin film (catalyst layer) with a film thickness of 3 nm.
[0238] Next, CNTs were formed on the substrate using a CVD device (reaction chamber size: diameter 30 mm, heating length 360 mm). Specifically, the prepared substrate was placed in a furnace maintained at a temperature of 750°C and a pressure of 1.02×10 5 Pa CVD device, and He: 100 sccm, H2: 900 sccm were introduced into the reaction chamber for 6 minutes. As a result, the CNT synthesis catalyst (iron) was reduced, and the micronization was promoted to a state suitable for the growth of single-walled CNTs (a state in which a plurality of nano-sized catalyst microparticles were formed on the base layer) (forming process). In addition, the density of the catalyst microparticles at this time was adjusted to 1×10 12 ~1×10 14 Pieces / cm 2 Then, the furnace temperature was maintained at 750°C and the pressure was maintained at 1.02×10 5 He: 850 sccm, C2H4: 59 sccm, and H2O: 300 ppm in concentration were supplied to the reaction chamber in the state of Pa for 5 minutes. Thus, single-walled CNTs grew from each catalyst fine particle (CNT growth step).
[0239] After the CNT growth step was completed, only He: 1000 sccm was supplied into the reaction chamber, and the remaining raw material gas and catalyst activator were removed. Thus, a substrate with CNTs formed on the surface was obtained.
[0240] Then, the CNTs grown on the substrate are peeled off from the surface of the obtained substrate. Specifically, the CNTs are peeled off using a plastic scraper having a sharp portion. During the peeling, the sharp portion of the scraper is brought into contact with the boundary between the CNTs and the substrate, and the sharp portion is moved along the surface of the substrate in a manner to shave off the CNTs from the substrate. Thus, the CNTs are peeled off from the substrate to obtain a used substrate.
[0241] [Preparation of recycled substrate]
[0242] Next, the used substrate obtained was immersed in water and cleaned for 5 minutes using an immersion ultrasonic cleaning machine 400G (output power 400W, oscillation frequency 38kHz) manufactured by Kaijie Co., Ltd. to obtain a reused substrate (initialization process). Then, the surface of the substrate after ultrasonic cleaning was washed with water, and then air was sprayed and dried (cleaning process). Then, the contact angle between the surface of the substrate and water before and after cleaning was measured using an automatic contact angle measuring instrument DMs-601 manufactured by Kyowa Interface Chemical Co., Ltd. The result showed that the contact angle before cleaning was 79°, while the contact angle after cleaning was 65°, confirming that the dirt on the substrate could be removed.
[0243] [Preparation of catalyst substrate for CNT growth]
[0244] On the surface of the recycled substrate, an alumina thin film (underlayer) and an iron thin film (catalyst layer) were formed by dip coating under the same conditions as above, thereby preparing a catalyst substrate for CNT growth.
[0245] [Synthesis of CNT]
[0246] Using the obtained CNT growth catalyst substrate, CNTs were formed on the substrate using the above-mentioned CVD apparatus under the same conditions as above. The obtained CNTs were referred to as CNTs (1).
[0247] In the Raman spectroscopic measurement of CNT (1), in single-walled CNT, the characteristic 100 cm -1 ~300cm -1 The spectrum of radial breathing mode (RBM) was observed in the low frequency region of CNT (1). In addition, the D' band of CNT (1) was not observed.
[0248] In addition, for CNT (1), the BET specific surface area, G / D ratio, the ratio of the number of single-walled CNTs to the total number of CNTs, the average diameter, the oxygen atomic ratio, and the average length were determined.
[0249] [Oxidation treatment]
[0250] 0.1 g of CNT (1) was added to 250 mL of a nitric acid (HNO3) aqueous solution having a concentration of 69 mass % (15.6 M) to prepare a mixed solution. The mixed solution was stirred at room temperature (about 25° C.) for 8 hours. Furthermore, a mantle-type resistance heater was used to raise the heater temperature to 180° C., and the nitric acid aqueous solution was refluxed for 6 hours at a liquid temperature of 123° C., and the CNT (1) contained in the mixed solution was oxidized to obtain a mixed solution containing oxidized CNT (1).
[0251] [Preparation of Oxidized CNT Dispersion]
[0252] Then, 1800 mL of deionized water was added to the mixed solution containing oxidized CNT (1) for dilution. After standing for 15 minutes to allow the oxidized CNT (1) to precipitate, the supernatant was removed. Then, deionized water was added to make the solution volume 1800 mL. A 0.1% ammonia solution was added to the obtained liquid as a neutralizer to adjust the pH of the liquid to 7.1. Then, ultrasonic treatment was performed for 2 hours using an ultrasonic irradiator to obtain an oxidized CNT (1) dispersion.
[0253] The absorbance ratio was calculated using the obtained oxidized CNT (1) dispersion liquid, and the dispersion stability was evaluated. The results are shown in Table 2.
[0254] In addition, the oxidized CNT (1) in the oxidized CNT (1) dispersion was filtered and dried. Then, for the dried oxidized CNT (1), the D' band, G / D' ratio, G / D ratio, the ratio of the number of oxidized single-walled CNTs to the total number of oxidized CNTs, the average diameter, the oxygen atomic ratio, and the average length were calculated. The single-wall ratio change rate and the average diameter change rate were then calculated. The results are shown in Table 2.
[0255] (Example 2)
[0256] <Synthesis of CNTs using recycled substrate>
[0257] [Synthesis of CNT]
[0258] Using the recycled substrate prepared in Example 1, the growth of CNTs using a CVD device was repeated in the same manner as in Example 1 to obtain CNTs (2).
[0259] In the Raman spectroscopic measurement of CNT (2), in single-walled CNT, the characteristic 100 cm -1 ~300cm -1 The spectrum of radial breathing mode (RBM) was observed in the low frequency region of CNT (2). In addition, the D' band of CNT (2) was not observed.
[0260] For CNT (2), the BET specific surface area, G / D ratio, the ratio of the number of single-walled CNTs to the total number of CNTs, the average diameter, the oxygen atomic ratio, and the average length were determined.
[0261] [Oxidation treatment]
[0262] 0.1 g of CNT (2) was added to 250 mL of a nitric acid (HNO3) aqueous solution having a concentration of 55% by mass (12.0 M) to prepare a mixed solution. The mixed solution was stirred at room temperature (about 25° C.) for 8 hours. Furthermore, a mantle-type resistance heater was used to raise the temperature of the heater to 180° C., and the nitric acid aqueous solution was refluxed for 12 hours at a liquid temperature of 117° C., and the CNT (2) contained in the mixed solution was oxidized to obtain a mixed solution containing oxidized CNT (2).
[0263] [Preparation of Oxidized CNT Dispersion]
[0264] The obtained mixed solution containing oxidized CNT (2) was subjected to the same operation as in Example 1 to obtain an oxidized CNT (2) dispersion.
[0265] Using the obtained oxidized CNT (2) dispersion, various measurements and evaluations were performed in the same manner as in Example 1. The results are shown in Table 2.
[0266] (Comparative Example 1)
[0267] <Synthesis of CNTs using raw substrate>
[0268] [Synthesis of CNT]
[0269] CNTs (3) were synthesized by synthesizing CNTs under the following conditions according to the super growth method described in Japanese Patent No. 4621896.
[0270] Carbon compounds as raw material compounds: Ethylene
[0271] Environment (carrier gas): Helium, hydrogen mixed gas
[0272] Catalyst activating substance: water vapor
[0273] Catalyst layer: Alumina film (base layer) and iron film (catalyst layer)
[0274] Original base material: SUS430
[0275] In the Raman spectroscopic measurement of CNT (3), in single-walled CNT, the characteristic 100 cm -1 ~300cm -1The spectrum of radial breathing mode (RBM) was observed in the low frequency region of CNT (3). In addition, the D' band of CNT (3) was not observed.
[0276] For CNT (3), the BET specific surface area, G / D ratio, the ratio of the number of single-walled CNTs to the total number of CNTs, the average diameter, the oxygen atomic ratio, and the average length were determined.
[0277] [Oxidation treatment]
[0278] 0.1 g of CNT (3) was added to 250 mL of a 39% by mass (7.7 M) nitric acid (HNO3) aqueous solution to prepare a mixed solution. The mixed solution was stirred at room temperature (about 25°C) for 8 hours. Furthermore, a mantle-type resistance heater was used to raise the heater temperature to 125°C, and the nitric acid aqueous solution was refluxed for 6 hours at a liquid temperature of 100°C, and the CNT (3) contained in the mixed solution was oxidized to obtain a mixed solution containing oxidized CNT (3).
[0279] [Preparation of Oxidized CNT Dispersion]
[0280] The obtained mixed solution containing oxidized CNT (3) was subjected to the same operation as in Example 1 to obtain an oxidized CNT (3) dispersion.
[0281] Using the obtained oxidized CNT (3) dispersion, various measurements and evaluations were performed in the same manner as in Example 1. The results are shown in Table 2.
[0282] (Comparative Example 2)
[0283] The same operation as in Comparative Example 1 was performed except that CNT (4) synthesized by the eDips method (manufactured by Meijo Nano Carbon Co., Ltd., "EC2.0P") was used instead of CNT (3) to obtain an oxidized CNT (4) dispersion. Then, various measurements and evaluations were performed in the same manner as in Comparative Example 1 using the obtained oxidized CNT (4) dispersion. The results are shown in Table 2.
[0284] [Table 2]
[0285]
[0286] As can be seen from Table 2, in Examples 1 and 2 using CNTs having predetermined properties, oxidized CNTs having excellent dispersibility and dispersion stability in water can be obtained.
[0287] On the other hand, it was found that in Comparative Examples 1 and 2 using CNTs not having the predetermined properties, oxidized CNTs excellent in dispersibility and dispersion stability in water could not be obtained.
[0288] Industrial Applicability
[0289] According to the present invention, it is possible to provide an oxidized CNT having excellent dispersibility and dispersion stability in water and a method for producing the same.
Claims
1. An oxidized carbon nanotube comprising an oxidized single-walled carbon nanotube, wherein the number of the oxidized single-walled carbon nanotubes accounts for more than 50% of the total number of the oxidized carbon nanotubes, The oxidized carbon nanotubes have a D' band in the Raman spectrum. Furthermore, the oxidized carbon nanotubes have a plurality of oxidized edge portions. The oxidized carbon nanotubes are obtained by subjecting carbon nanotubes including single-walled carbon nanotubes to an oxidation treatment process, and the BET specific surface area of the carbon nanotubes is greater than 1300 m 2 / g.
2. The oxidized carbon nanotube according to claim 1, wherein: The average diameter of the oxidized carbon nanotubes is greater than or equal to 3.5 nm and less than or equal to 5 nm.
3. The oxidized carbon nanotube according to claim 1 or 2, wherein: The oxygen atomic ratio of the oxidized carbon nanotubes is greater than 15 at %.
4. The oxidized carbon nanotube according to claim 1 or 2, wherein: The average length of the oxidized carbon nanotubes is greater than or equal to 30 nm and less than or equal to 120 nm.
5. A method for producing oxidized carbon nanotubes, the method for producing oxidized carbon nanotubes according to any one of claims 1 to 4, comprising an oxidation treatment step of oxidizing carbon nanotubes including single-walled carbon nanotubes, wherein the carbon nanotubes have a BET specific surface area greater than 1300 m 2 / g.
6. The method for producing oxidized carbon nanotubes according to claim 5, wherein: The carbon nanotubes have a G / D ratio greater than 3.0 and less than 10.
7. The method for producing oxidized carbon nanotubes according to claim 5 or 6, wherein: In the oxidation treatment step, the oxidation treatment is performed using an aqueous nitric acid solution having a concentration greater than 40% by mass.
8. The method for producing oxidized carbon nanotubes according to claim 7, wherein: In the oxidation treatment step, the mixture including the carbon nanotubes and the nitric acid aqueous solution is refluxed at a temperature of ±5° C. of the azeotropic point of the nitric acid aqueous solution.
9. The method for producing oxidized carbon nanotubes according to claim 5 or 6, wherein: In the oxidation treatment step, the carbon nanotubes are oxidized so that the single-wall ratio change rate represented by the following formula (1) becomes 90% or less. Single wall ratio change rate = SGCNT A / SGCNT B =100(%)…Formula (1) In formula (1), SGCNT A It represents the ratio of the number of oxidized single-walled carbon nanotubes to the total number of oxidized carbon nanotubes. B It indicates the ratio of the number of single-walled carbon nanotubes to the total number of carbon nanotubes.
10. The method for producing oxidized carbon nanotubes according to claim 5 or 6, wherein: In the oxidation treatment step, the carbon nanotubes are oxidized so that the average diameter change rate represented by the following formula (2) is greater than 100%. Average diameter change rate = CNT DA / CNT DB ×100(%)…Formula (2) In formula (2), CNT DA represents the average diameter of oxidized carbon nanotubes, CNT DB represents the average diameter of carbon nanotubes.
Citation Information
Patent Citations
Production method of reused substrate, and production method of catalyst substrate for producing carbon nanotube
JP2015188811A
Single-layer carbon nanotube and alinged single-layer carbon nanotube bulk structure, and their production process, production apparatus and use
WO2006011655A1
Fibrous carbon nanostructure dispersion and method for producing same, and fibrous carbon nanostructure
WO2018180901A1
Carbon nanotubes, dispersion liquid thereof, carbon nanotube-containing film and composition material