Treatment method of high talc molybdenum ore dressing return water

By adding a mixture of oxidizing bactericides and demulsifiers and flocculants in the talc-type molybdenum ore beneficiation process, the problem of processing fine-grained minerals and oily molybdenum collectors in the return water is solved, and the flotation effect and recovery rate are improved, achieving Efficient return water recycling.

CN115925164BActive Publication Date: 2024-10-15CHINA MINMETALS CHANGSHA MINING RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211541671.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-01
Publication Date
2024-10-15
Estimated Expiration
2042-12-01

AI Technical Summary

Technical Problem

In the beneficiation of talc-type molybdenum ore, the presence of fine-grained minerals and oily molybdenum collectors in the return water makes flotation separation more difficult and degrades slowly, resulting in a high molybdenum loss rate. It is difficult to effectively treat it with existing technology and affects the circulation of the return water. use.

Method used

Add a mixture of oxidizing bactericide and demulsifier to the tailings pump pool for high talc-type molybdenum ore beneficiation, and add flocculant at the pipeline pump outlet of the tailings pump pool to remove fine minerals in the return water through synergy. Use it with oil molybdenum collector to improve the quality of return water.

Benefits of technology

It effectively improves the quality of return water, reduces the molybdenum loss rate, improves the grade and recovery rate of molybdenum concentrate, reduces the complexity of the mineral processing process, and creates economic benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115925164B_ABST
    Figure CN115925164B_ABST
Patent Text Reader

Abstract

The present invention provides a method for treating the return water of high-talc molybdenum ore beneficiation. A mixture of an oxidizing bactericide and a demulsifier is added to the tailings pump pool of the high-talc molybdenum ore beneficiation; and a flocculant is added at the outlet of the pipeline pump of the tailings pump pool. After the sedimentation of the tailings pond, the recyclable beneficiation return water is obtained. The oxidizing bactericide will reduce the electrostatic repulsion between oil collectors, which is conducive to the aggregation of collectors; it will also oxidize the collectors on the surface of fine mineral particles, strengthen the contact between the demulsifier's surfactant and the oil-water mixture, and promote the emulsification effect of the demulsifier. Under the synergistic effect of the oxidizing bactericide and the demulsifier, the present invention achieves the effect of removing fine mineral particles and oil collectors in the return water, improves the quality of the return water, eliminates the difficulty and adverse effects of the return water return operation on the molybdenum ore flotation process in the prior art, and thus improves the grade and recovery rate of the molybdenum concentrate obtained by flotation, creating good economic benefits for the enterprise.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ore dressing return water treatment, and in particular to a method for treating high-talc molybdenum ore dressing return water. Background Art

[0002] Due to the serious shortage of water resources and the requirements of environmental protection, it is necessary to return the water used in mineral processing to the mineral processing process for reuse, and it has been paid more and more attention; the water returned for use is called return water or circulating water. In the flotation of talc-type molybdenum ore, since talc and molybdenite have similar crystal structures and floatability, flotation separation is difficult, and talc is very easy to muddy during grinding. The muddy gangue particles will produce a large surface energy, forming a mud cover on useful minerals, preventing the collector from contacting with useful minerals, and at the same time making the viscosity of the slurry too high, the aeration conditions worsen, the flotation environment chaotic, and easy to produce cover, heterogeneous coagulation and self-coagulation, so that useful minerals and muddy gangue particles and flotation reagents enter the return water, which not only increases the difficulty of flotation recovery of molybdenum minerals, but also makes the components in the return water complicated, increasing the difficulty of reuse.

[0003] Studies have shown that in the beneficiation process of talc-type molybdenum ore, one of the most important factors affecting the molybdenum loss rate in the talc removal operation is water quality. A large amount of fine-grained minerals and oily molybdenum collectors and other substances remain in the return water of molybdenum ore; the fine-grained minerals are fine in size and extremely low in grade, and are easily covered on the surface of coarse-grained concentrate when the return water is recycled, seriously deteriorating the flotation effect; the oily molybdenum collector is relatively stable in nature and has a slow degradation rate, which will cause a sharp increase in the molybdenum loss rate in the talc removal operation, resulting in a low recovery rate in the molybdenum selection operation. Therefore, how to treat the return water of high-talc molybdenum ore is of great significance to achieve efficient flotation of molybdenum ore and improve the grade and recovery rate of molybdenum concentrate.

[0004] The invention patent (application number CN 201510129430.8) discloses a process and device for recycling wastewater from copper-molybdenum separation. The device collects overflow water and filtered water in the copper-molybdenum separation process in a return water tank, removes residual reagents that are not conducive to copper-molybdenum separation by adding activated carbon to adsorb flotation reagents in the return water tank, and then presses the return water into the return water pipe through a water pump next to the return water tank and returns it to the separation flotation operation for recycling; although the device realizes the treatment of return water and returns it to flotation for use, in the flotation of talc-type molybdenum ore, many types of reagents are used, and the reagents affect each other, and the content of fine-grained minerals in the return water is high. It is difficult to eliminate the adverse effects of the return water on the subsequent molybdenum selection operation by only using activated carbon for adsorption treatment. At present, there is no special treatment method for fine-grained minerals and oil-based molybdenum collectors in the return water of high-talc molybdenum ore.

[0005] In view of this, it is necessary to design an improved method for treating the return water of high-talc molybdenum ore dressing to solve the above problems. Summary of the invention

[0006] The object of the present invention is to provide a method for treating return water from high-talc molybdenum ore dressing. A mixture of an oxidizing fungicide and a demulsifier is added to a tailings pump pool of high-talc molybdenum ore dressing. Under the synergistic effect of the two, the fine-grained minerals and oil-based molybdenum collectors in the return water are removed, so as to eliminate the adverse effects of the return water on subsequent molybdenum dressing operations, thereby improving the grade and recovery rate of the molybdenum concentrate obtained by flotation.

[0007] To achieve the above-mentioned object of the invention, the present invention provides a method for treating high-talc molybdenum ore dressing return water, comprising the following steps:

[0008] S1. Adding a mixture of an oxidizing bactericide and a demulsifier into a tailings pump pool of a high-talc molybdenum ore dressing process; the addition amount of the mixture is 200-600 g / t; the mass ratio of the oxidizing bactericide to the demulsifier in the mixture is 1:(0.8-1.2);

[0009] S2. Add flocculant at the outlet of the pipeline pump of the tailings pump pool, and obtain recyclable mineral processing return water through the sedimentation of the tailings pond.

[0010] As a further improvement of the present invention, in step S1, the oxidizing bactericide includes one of a hypochlorite bactericide or a polyquaternary ammonium salt bactericide.

[0011] As a further improvement of the present invention, the oxidizing fungicide is a polyquaternary ammonium salt fungicide, and the addition amount thereof is 100 to 300 g / t.

[0012] As a further improvement of the present invention, in step S2, the flocculant includes one or more of polyacrylamide, lime, aluminum sulfate, and alum.

[0013] As a further improvement of the present invention, the flocculant is polyacrylamide, and the addition amount thereof is 10 to 30 g / t.

[0014] As a further improvement of the present invention, when the flocculant is one or more of lime, aluminum sulfate and alum, the addition amount thereof is 500 to 3000 g / t.

[0015] As a further improvement of the present invention, the hypochlorite disinfectant includes one of sodium hypochlorite and calcium hypochlorite or a mixture of the two.

[0016] As a further improvement of the present invention, in step S1, the demulsifier includes one or a mixture of two of polyoxyethylene polyoxypropylene octadecyl alcohol ether and polyoxyethylene polyoxypropylene polyether.

[0017] As a further improvement of the present invention, the talc in the high-talc type molybdenum ore is 10% to 35% by mass.

[0018] As a further improvement of the present invention, in step S1, in the high-talc molybdenum ore beneficiation process, the reagent used includes an oil-based molybdenum collector; the oil-based molybdenum collector includes kerosene, diesel, or a mixture of both.

[0019] The beneficial effects of the present invention are:

[0020] 1. The present invention provides a method for treating the return water of high-talc molybdenum ore beneficiation, wherein a mixture of an oxidizing bactericide and a demulsifier is added to the tailings pump pool of the high-talc molybdenum ore beneficiation, and a flocculant is added at the outlet of the pipeline pump of the tailings pump pool, and the return water of the beneficiation that can be recycled is obtained through the sedimentation of the tailings pond. Under the synergistic effect of the oxidizing bactericide and the demulsifier, the present invention achieves the effect of removing fine-grained minerals and oil-based molybdenum collectors in the return water, improves the quality of the return water, eliminates the difficulty and adverse effects of the return water re-return operation on the molybdenum ore flotation process in the prior art, and thus improves the grade and recovery rate of the molybdenum concentrate obtained by flotation.

[0021] 2. The oxidizing fungicide used in the present invention can not only eliminate the influence of microorganisms in the return water, but also reduce the electrostatic repulsion between oil collectors, which is conducive to the aggregation of oil collectors and promotes the emulsification effect of demulsifiers. In addition, oil collectors are easy to adhere to the surface of fine minerals, affecting the emulsification of collectors and the subsequent contact between fine minerals and flocculants, while the oxidizing fungicide will oxidize the collectors on the surface of fine minerals, which can strengthen the contact between the demulsifier's surface active substances and the oil-water mixture, thereby promoting the emulsification effect of the demulsifier. Therefore, the mixed use of oxidizing fungicides and demulsifiers can play a synergistic enhancement effect, thereby improving the treatment effect of oil collectors and fine minerals in the return water.

[0022] 3. The method for treating the high-talc molybdenum ore dressing return water of the present invention can not only eliminate the molybdenum collector residual in the return water, but also will not cause adverse effects on the subsequent molybdenum dressing operations; after the obtained return water is returned to the molybdenum ore flotation process, the talc removal operation section is obtained to achieve a near-clean water effect, which greatly reduces the molybdenum loss rate in this stage, effectively improves the ore dressing index, and creates good economic benefits for the enterprise.

[0023] 4. The treatment method of the present invention is simple and easy to implement, and has no adverse interference with the normal flotation process of high-talc molybdenum ore in the ore dressing plant. It is only operated at the tailings pump pool and its pipeline pump outlet. It has the characteristics of high practicality, low cost and high universality. It is suitable for the flotation process of high-talc molybdenum ore in existing ore dressing plants, and provides a new method for the treatment and recycling of its return water. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The present invention is a process flow chart of the method for treating the high-talc molybdenum ore dressing return water.

[0025] Figure 2 This is a flow chart of the application of mineral processing return water obtained in Example 1 of the present invention. DETAILED DESCRIPTION

[0026] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0027] It should also be noted that, in order to avoid obscuring the present invention due to unnecessary details, only structures and / or processing steps closely related to the scheme of the present invention are shown in the drawings, while other details that are not closely related to the present invention are omitted.

[0028] In addition, it should be noted that the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.

[0029] A method for treating high-talc molybdenum ore dressing return water comprises the following steps:

[0030] S1. Add a mixture of an oxidizing fungicide and a demulsifier into the tailings pump pool of a high-talc molybdenum ore dressing process; the addition amount of the mixture is 200-600 g / t; the mass ratio of the oxidizing fungicide to the demulsifier in the mixture is 1:(0.8-1.2);

[0031] S2. Add flocculant at the outlet of the pipeline pump of the tailings pump pool, and obtain recyclable mineral processing return water through the sedimentation of the tailings pond.

[0032] In particular, the oxidizing bactericide includes one of a hypochlorite bactericide or a polyquaternary ammonium salt bactericide. The oxidizing bactericide used in the present invention can not only eliminate the influence of microorganisms in the return water, but also reduce the electrostatic repulsion between oil collectors, which is conducive to the aggregation of oil collectors and promotes the emulsification effect of demulsifiers; in addition, oil collectors are easily attached to the surface of fine minerals, affecting the emulsification of collectors and the subsequent contact between fine minerals and flocculants, while the oxidizing bactericide will oxidize the collectors on the surface of fine minerals, which can strengthen the contact between the demulsifier surface active substances and the oil-water mixture, thereby promoting the emulsification effect of the demulsifier. Therefore, the mixed use of oxidizing bactericides and demulsifiers can play a synergistic enhancement effect, thereby improving the treatment effect of oil collectors and fine minerals in the return water.

[0033] Preferably, the oxidizing bactericide is a polyquaternary ammonium salt bactericide, and the addition amount thereof is 100 to 300 g / t. When the polyquaternary ammonium salt is used as a bactericide, it not only has the above-mentioned effects, but also has the effect of emulsifying the oil collector, further realizing the effective removal of the oil collector in the return water.

[0034] In some specific embodiments, the hypochlorite sterilant includes sodium hypochlorite, calcium hypochlorite, or a mixture of the two.

[0035] In some specific embodiments, the demulsifier includes one or a mixture of polyoxyethylene polyoxypropylene octadecyl alcohol ether, polyoxyethylene polyoxypropylene polyether.

[0036] It should be noted that in other fields, such as oil production plants or oil field wastewater, demulsifiers are usually used to reduce the oil-water interfacial tension, convert organic oil-soluble salts into water-soluble salts, and make them easy to enrich, forming large droplets, and finally leaving the oil phase and entering the water phase, completing the oil-water separation of oil products, and achieving the purpose of desalting, dehydrating and demulsifying. However, this method is only applicable to the treatment of wastewater with high oil content; in the field of return water treatment of molybdenum ore dressing, the content of oil molybdenum collector is about 10ppm, which is hundreds to tens of thousands times lower than that in wastewater such as oil fields. If a single demulsifier in the existing technology is also used, it is difficult to achieve effective removal.

[0037] Specifically, in step S2, the flocculant includes one or more of polyacrylamide, lime, aluminum sulfate, and alum. When the flocculant is one or more of lime, aluminum sulfate, and alum, the addition amount thereof is 500 to 3000 g / t. When the flocculant is polyacrylamide, the addition amount thereof is 10 to 30 g / t. As an organic flocculant, polyacrylamide has a high molecular weight and a high flocculation effect, so only a small amount needs to be added to achieve a good flocculation effect.

[0038] It should be noted that the unit of g / t for the addition amount of the above-mentioned oxidizing fungicide, demulsifier, mixture of the two and flocculant indicates the tons of tailings slurry corresponding to the grams of the added substance.

[0039] The method for treating the high-talc molybdenum ore beneficiation return water of the present invention is specifically aimed at the molybdenum ore in which the talc in the high-talc molybdenum ore is 10% to 35% by mass. In the actual flotation process of such molybdenum ore, the reagents used include oil molybdenum collectors, and the oil molybdenum collectors include one or a mixture of two of kerosene and diesel. The flotation of the high-talc molybdenum ore is affected by the excess oil molybdenum collector in the return water, and the molybdenum loss rate is high when the talc is removed. The ore dressing plant often tries its best to control the amount of talc removed, resulting in part of the talc entering the molybdenum flotation system, which reduces the final molybdenum concentrate grade and recovery rate to a certain extent. The present invention solves the influence of the return water on the talc removal operation, so that the flotation process can increase the amount of talc removed as much as possible to eliminate the influence of talc on the molybdenum flotation, and can effectively improve the final molybdenum concentrate grade and recovery rate.

[0040] See also Figure 1 As shown, it is a process flow chart of the treatment method of high talc molybdenum ore beneficiation return water of the present invention. It can be seen that a mixture of an oxidizing bactericide and a demulsifier is added to the tailings pump pool of the high talc molybdenum ore beneficiation, and a flocculant is added at the outlet of the pipeline pump of the tailings pump pool. After the sedimentation of the tailings pond, recyclable beneficiation return water is obtained; and the treated return water is returned to the beneficiation process for recycling. The treatment method is simple and easy to implement, and has no adverse interference with the normal high talc molybdenum ore flotation process of the beneficiation plant. It is only operated at the outlet of the tailings pump pool and its pipeline pump. It has the characteristics of high practicality, low cost and high universality. It is suitable for the flotation process of high talc molybdenum ore in existing beneficiation plants, and provides a new method for the treatment and recycling of its return water.

[0041] Example 1

[0042] This embodiment provides a method for treating high-talc molybdenum ore dressing return water, comprising the following steps:

[0043] S1. In the tailings pump pool during the beneficiation of high-talc molybdenum ore, a mixture of polyquaternary ammonium salt and polyoxyethylene polyoxypropylene octadecyl alcohol ether is added, and the addition amount of both is 300g / t;

[0044] S2. Add 20g / t of polyacrylamide at the outlet of the pipeline pump of the tailings pump pool, and obtain recyclable mineral processing return water through the sedimentation of the tailings pond;

[0045] S3, the beneficiation return water obtained in step S2 is used for the preliminary talc removal operation, the specific process is as follows Figure 2 shown.

[0046] Comparative Example 1

[0047] In Comparative Example 1, the return water was not treated in any way and was directly returned for use in the preliminary talc removal operation.

[0048] Comparative Example 2

[0049] Comparative Example 2 provides a method for treating high-talc molybdenum ore dressing return water. Compared with Example 1, the difference is that the treatment of step S1 is not performed, and the rest is roughly the same as Example 1, which will not be repeated here.

[0050] Comparative Example 3

[0051] Comparative Example 3 provides a method for treating high-talc molybdenum ore dressing return water. Compared with Example 1, the difference is that in step S1, polyquaternary ammonium salt and polyoxyethylene polyoxypropylene octadecyl alcohol ether are separately added to the tailings pump pool for treatment, and the rest is roughly the same as Example 1 and will not be repeated here.

[0052] The influence of the ore dressing return water of Example 1 and Comparative Examples 1 to 3 on the molybdenum loss rate in the talc removal stage was detected and compared with the molybdenum loss rate of the talc removal operation using clean water in advance. The results are shown in the following table.

[0053] Table 1 Related test results of Example 1 and Comparative Examples 1 to 3

[0054] Molybdenum grade of talc rough concentrate (%) Talc rough concentrate loss rate (%) Shimizu 0.032 1.33 Example 1 0.033 1.49 Comparative Example 1 0.328 15.24 Comparative Example 2 0.263 13.47 Comparative Example 3 0.178 7.18

[0055] As can be seen from Table 1, the molybdenum grade and loss rate of the talc rough concentrate obtained by the return water treated by the scheme of Example 1 in the pre-talc removal operation of the molybdenum ore flotation are similar to those of directly using clean water, which greatly reduces the molybdenum loss rate and creates good economic benefits for the enterprise. The return water utilization method of Examples 1 to 2 has very high molybdenum grade and loss rate in the talc removal operation. In Example 3, the oxidizing bactericide and demulsifier are added separately, which reduces the molybdenum loss rate, but the effect is still not ideal compared with Example 1 and the clean water group. It can be seen that the mixed addition method of the oxidizing bactericide and the demulsifier has a synergistic effect, which is beneficial to improve the quality of the return water and eliminate the adverse effects of the return water on the flotation of the molybdenum ore.

[0056] Example 2

[0057] The present embodiment provides a method for treating return water from ore dressing of high-talc molybdenum ore. Compared with Example 1, the difference lies in that in step S1, 100 g / t of sodium hypochlorite is used instead of polyquaternary ammonium salt, 250 g / t of polyoxyethylene polyoxypropylene polyether is used instead of polyoxyethylene polyoxypropylene octadecyl alcohol ether, and in step S2, 1000 g / t of lime is used instead of polyacrylamide; the rest is roughly the same as Example 1 and will not be repeated here.

[0058] Comparative Example 4

[0059] Comparative Example 4 provides a method for treating high-talc molybdenum ore dressing return water. Compared with Example 2, the difference is that in step S1, sodium hypochlorite and polyoxyethylene polyoxypropylene polyether are separately added to the tailings pump pool for treatment, and the rest is roughly the same as Example 2 and will not be repeated here.

[0060] Example 3

[0061] The present embodiment provides a method for treating return water from high-talc molybdenum ore dressing. Compared with Example 1, the difference lies in that in step S1, calcium hypochlorite is used instead of polyquaternary ammonium salt, the addition amount of ethylene glycol polyoxypropylene octadecyl alcohol ether is 100 g / t, and in step S2, 2000 g / t of alum is used instead of polyacrylamide; the rest is roughly the same as Example 1 and will not be repeated here.

[0062] Comparative Example 5

[0063] Comparative Example 5 provides a method for treating high-talc molybdenum ore dressing return water. Compared with Example 3, the difference is that in step S1, calcium hypochlorite and oxyethylene polyoxypropylene octadecyl ether are separately added to the tailings pump pool for treatment, and the rest is roughly the same as Example 3 and will not be repeated here.

[0064] The influence of the beneficiation return water of Examples 2-3 and Comparative Examples 4-5 on the molybdenum loss rate in the talc removal stage was detected and compared with the molybdenum loss rate of the talc removal operation using clean water in advance. The results are shown in the following table.

[0065] Table 2 Related test results of Examples 2-3 and Comparative Examples 4-5

[0066] Molybdenum grade of talc rough concentrate (%) Talc rough concentrate loss rate (%) Shimizu 0.032 1.33 Example 2 0.042 1.89 Example 3 0.035 1.53 Comparative Example 4 0.183 7.57 Comparative Example 5 0.196 8.45

[0067] As shown in Table 2, the mixed addition of oxidizing bactericide and demulsifier in Examples 2 and 3 has a synergistic effect, reducing the molybdenum loss rate in the pre-talc removal operation; in Examples 1 to 3, the molybdenum grade and loss rate of the talc rough concentrate in Example 1 are the lowest. In Comparative Examples 4 to 5, the loss rate of the talc rough concentrate is still above 7% by adding the oxidizing bactericide and demulsifier separately.

[0068] In summary, the present invention provides a method for treating high-talc molybdenum ore dressing return water, wherein a mixture of an oxidizing bactericide and a demulsifier is added to the tailings pump pool of the high-talc molybdenum ore dressing, and a flocculant is added at the outlet of the pipeline pump of the tailings pump pool, and a recyclable dressing return water is obtained through the sedimentation of the tailings pond. Among them, the oxidizing bactericide can not only eliminate the influence of microorganisms in the return water, but also reduce the electrostatic repulsion between oil collectors, which is conducive to the aggregation of oil collectors and promotes the emulsification effect of demulsifiers; in addition, the oxidizing bactericide will oxidize the oil collectors on the surface of fine-grained minerals, which can strengthen the contact between the demulsifier surfactant and the oil-water mixture, thereby promoting the emulsification effect of the demulsifier. Therefore, the mixed use of the oxidizing bactericide and the demulsifier can play a synergistic enhancement effect, thereby improving the treatment effect of the oil collector and fine-grained minerals in the return water. Under the synergistic effect of the oxidizing bactericide and the demulsifier, the present invention achieves the effect of removing fine-particle minerals and oil-based molybdenum collectors in the return water, improves the quality of the return water, eliminates the difficulty and adverse effects of the return water return operation on the molybdenum ore flotation process in the prior art, thereby improving the grade and recovery rate of the molybdenum concentrate obtained by flotation, effectively improving the mineral processing indicators, and creating good economic benefits for the enterprise.

[0069] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention.

Claims

1. A method for treating high-talc molybdenum ore dressing return water, characterized in that: The following steps are involved: S1. Add a mixture of an oxidizing fungicide and a demulsifier into a tailings pump pool of a high-talc molybdenum ore dressing process; the addition amount of the mixture is 200-600 g / t; the mass ratio of the oxidizing fungicide to the demulsifier in the mixture is 1:(0.8-1.2); the talc in the high-talc molybdenum ore is 10%-35% by mass; the oxidizing fungicide includes one of a hypochlorite fungicide or a polyquaternary ammonium salt fungicide, and the demulsifier includes one of polyoxyethylene polyoxypropylene octadecyl alcohol ether and polyoxyethylene polyoxypropylene polyether, or a mixture of two thereof; S2. Add flocculant at the outlet of the pipeline pump of the tailings pump pool, and obtain recyclable mineral processing return water through the sedimentation of the tailings pond.

2. The method for treating high talc type molybdenum ore dressing return water according to claim 1, characterized in that: The oxidizing bactericide is a polyquaternary ammonium salt bactericide, and the addition amount thereof is 100-300 g / t.

3. The method for treating high talc type molybdenum ore dressing return water according to claim 1, characterized in that: In step S2, the flocculant includes one or more of polyacrylamide, lime, aluminum sulfate, and alum.

4. The method for treating high talc type molybdenum ore dressing return water according to claim 3, characterized in that: The flocculant is polyacrylamide, and the addition amount thereof is 10-30 g / t.

5. The method for treating high talc type molybdenum ore dressing return water according to claim 3, characterized in that: When the flocculant is one or more of lime, aluminum sulfate and alum, the added amount is 500-3000 g / t.

6. The method for treating high talc type molybdenum ore dressing return water according to claim 1, characterized in that: The hypochlorite disinfectant includes one of sodium hypochlorite and calcium hypochlorite or a mixture of the two.

7. The method for treating high-talc molybdenum ore dressing return water according to claim 1, characterized in that: In step S1, in the high-talc molybdenum ore beneficiation process, the reagents used include oil-based molybdenum collectors; the oil-based molybdenum collectors include kerosene, diesel, or a mixture of both.