Wear-resistant coated glass and preparation method thereof
By combining silicon nitride base layer, silver plating layer, wear-resistant layer and protective layer on coated glass, a highly crosslinked wear-resistant layer and epoxy modified silicone resin are formed using materials such as silicon sol and modified nano zinc oxide. The protective layer was prepared by other materials, which solved the problem of insufficient corrosion resistance and wear resistance of coated glass, and achieved high light transmittance and wear resistance.
Patent Information
- Application Number
- CN202310083067.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-08
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-02-08
AI Technical Summary
The existing coated glass has poor corrosion resistance and is easily eroded by external environment, resulting in a reduced light transmittance. The silver-plated layer is easily scratched during transportation and installation, causing roughness of the glass surface and further reducing the light transmittance.
A wear-resistant coating glass structure consisting of silicon nitride base layer, silver plating layer, wear-resistant layer and protective layer. The wear-resistant layer is made of silicon sol, modified nano zinc oxide, silane coupling agent and other materials. Deposition by DC magnetron sputtering technology, the wear-resistant layer and protective layer are prepared from epoxy modified silicone resin, polytetrafluoroethylene micropowder and other materials, forming a highly crosslinked mesh structure to improve wear resistance and corrosion resistance.
It significantly improves the wear resistance and light transmittance of the coated glass, prevents friction and scratches of the silver-plated layer, and ensures high light transmittance while enhancing the resistance to erosion.
Smart Images

Figure BDA0004068050200000081
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of coated glass, and in particular relates to wear-resistant coated glass and a preparation method thereof. Background Art
[0002] Coated glass is coated with one or more layers of transparent thin films of metal, metal compound or non-metal compound on the glass surface by chemical vapor deposition, physical vapor deposition, plasma sputtering deposition, metal organic deposition and sol-gel method, so that the glass can have functions such as conductivity and anti-static. However, the corrosion resistance of this coating is poor and it is easily corroded by the external environment, resulting in reduced light transmittance of the glass. In the prior art, a silver plating layer is selected to improve the high light transmittance. Since silver is soft in texture, it is easily scratched by friction during transportation and installation, resulting in a rough glass surface, which also leads to reduced light transmittance of the glass. Summary of the invention
[0003] The object of the present invention is to provide a wear-resistant coated glass and a preparation method thereof, so as to solve the problems in the background technology.
[0004] The purpose of the present invention can be achieved through the following technical solutions:
[0005] A wear-resistant coated glass comprises a glass body, wherein a silicon nitride primer layer, a silver-plated layer, a wear-resistant layer and a protective layer are sequentially arranged on the surface of the glass body; the material of the wear-resistant layer is a wear-resistant coating; the material of the protective layer is a corrosion-resistant coating; the wear-resistant coating comprises the following raw materials in parts by weight: 9.4-15 parts of deionized water, 1-8 parts of silica sol, 1-1.2 parts of sulfuryl chloride, 5-8 parts of modified nano zinc oxide, 10-14 parts of mixed solution A, 2.8-3.3 parts of silane coupling agent KH-560, and 14-20 parts of isopropyl alcohol.
[0006] As a further embodiment of the present invention, the particle size of the silica sol is 12-15 nm.
[0007] As a further solution of the present invention, the modified nano zinc oxide comprises the following preparation steps:
[0008] After 10-12mL of stearic acid and 20-30mL of isopropanol are mixed and stirred evenly, 1-1.5g of nano zinc oxide is added, and the mixture is stirred for 1-1.2h at 18-20°C, and then allowed to stand for 30-40min, and the supernatant is removed to obtain modified nano zinc oxide. The modified nano zinc oxide is surface-modified by stearic acid, which reduces the surface activation energy of nano zinc oxide and improves its dispersibility in wear-resistant coatings; the modified nano zinc oxide has the characteristics of high transparency and low refractive index, is easy to be doped, can change the porosity and surface roughness of the coating system, and improves the light transmittance of the coating.
[0009] As a further embodiment of the present invention, the mixed solution A is prepared by mixing 3-isocyanatepropyltriethoxysilane and methyl orthosilicate in a mass ratio of 5-6.5:1-1.3.
[0010] As a further solution of the present invention, the wear-resistant coating comprises the following preparation steps:
[0011] Weigh the raw materials according to the formula, add deionized water, silica sol, sulfuryl chloride, and modified nano zinc oxide into the reaction container, drop the mixed solution A, react at 80-85°C for 30-45min, cool to 25±1.5°C, add silane coupling agent KH-560 and isopropanol, stir for 1-2h, and obtain the wear-resistant coating. 3-isocyanatepropyltriethoxysilane is hydrolyzed to generate silanol, and the silanol of the silica sol particles is further dehydrated and condensed with silanol to generate siloxane (SiOSi) covalent bonds, and finally form a highly cross-linked dense mesh or body structure through the curing process. The coating as a wear-resistant layer is beneficial to improving the wear resistance of the coating.
[0012] As a further embodiment of the present invention, the corrosion-resistant coating comprises the following preparation steps:
[0013] Step S1, dissolving epoxy resin E-44 in acetone, adding silicone resin TSR-144, silane coupling agent KH560, and dibutyltin dilaurate, heating to 80-90° C., reflux stirring for 1.5-2 h, fully mixing, cooling after reaction, and obtaining epoxy-modified silicone resin;
[0014] Step S2, after the epoxy modified silicone resin, polytetrafluoroethylene powder and defoamer BYK-141 are mixed and ground to a fineness of 25-30 μm, curing agent T-31 is added, and the mixture is stirred evenly to obtain a corrosion resistant coating. Polytetrafluoroethylene has structural characteristics such as high crystallinity, large relative molecular mass, no side chains in the molecule, high CF bond energy, and F atoms shielding the main chain, which improves the corrosion resistance and wear resistance of the coating.
[0015] As a further embodiment of the present invention, the mass ratio of the epoxy resin E-44, acetone, silicone resin TSR-144, silane coupling agent KH560, and dibutyltin dilaurate in step S1 is 40-50:40-50:20-30:2-3:1-1.2.
[0016] As a further solution of the present invention, the mass ratio of the epoxy-modified silicone resin, polytetrafluoroethylene powder, defoamer BYK-141, and curing agent T-31 in step S2 is 20-30:20-30:20-30:1-5.
[0017] As a further solution of the present invention, the method for preparing the wear-resistant coated glass comprises the following preparation steps:
[0018] Step 1: Prepare a silicon nitride base layer on the surface of the glass body by using a DC magnetron sputtering technique;
[0019] Step 2: preparing a silver-plated layer on the surface of the glass body by using a DC magnetron sputtering technique;
[0020] Step 3: Filter the wear-resistant coating with a 3 μm microporous filter membrane, add the wetting and leveling agent BYK-333 and mix, apply it on the surface of the silver-plated layer by flow coating, and after the surface is dry, dry it at a constant temperature of 40-50° C. for 1-2 hours to solidify the coating, and the wear-resistant layer is prepared;
[0021] Step 4: Spray the corrosion-resistant coating on the outside of the wear-resistant layer, dry it at 25±1.5°C for 24-30 hours to solidify the coating, and the protective layer is prepared to obtain a wear-resistant coated glass.
[0022] As a further solution of the present invention, the target material of the DC magnetron sputtering technology in step 1 is a silicon target, the functional gases are argon and nitrogen, the volume ratio of argon to nitrogen is 1-3:1-8, and the vacuum degree is 0.1-1.33Pa.
[0023] As a further solution of the present invention, the target material of the DC magnetron sputtering technology in step 2 is a silver target.
[0024] As a further solution of the present invention, the mass ratio of the wear-resistant coating in step three to the wetting and leveling agent BYK-333 is 100:0.3-0.4.
[0025] Beneficial effects of the present invention:
[0026] The present invention generates silanol by hydrolyzing 3-isocyanate propyl triethoxysilane, and further dehydrates and condenses the silanol of the silica sol particles to generate a silicon-oxygen-silicon (Si-OS i) covalent bond, and finally forms a highly cross-linked and dense network or body structure through a curing process. The material of the prepared wear-resistant layer is beneficial to improving the wear resistance of the glass, preventing the silver-plated layer from being scratched by friction, and ensuring the high light transmittance of the silver-plated layer of the coated glass.
[0027] The present invention modifies the surface of nano zinc oxide by using stearic acid, thereby reducing the surface activation energy of nano zinc oxide and improving its dispersibility in wear-resistant coatings; the modified nano zinc oxide has the characteristics of high transparency and low refractive index, is easy to be doped, can change the porosity and surface roughness of the coating system, and further improves the light transmittance of the glass;
[0028] The invention obtains the corrosion-resistant coating by mixing epoxy-modified organic silicon resin, polytetrafluoroethylene powder and defoamer BYK-141, grinding and mixing with curing agent T-31. The polytetrafluoroethylene has the structural characteristics of high crystallinity, large relative molecular mass, no side chain in the molecule, high CF bond energy and F atom shielding the main chain. The prepared protective layer material can improve the corrosion resistance of the wear-resistant layer, further improve the wear resistance of the wear-resistant layer, and ensure the high light transmittance of the glass. DETAILED DESCRIPTION
[0029] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] Example 1
[0031] A modified nano zinc oxide comprises the following preparation steps:
[0032] After 10 mL of stearic acid and 20 mL of isopropanol are mixed and stirred evenly, 1 g of nano zinc oxide is added, and the mixture is stirred for 1 hour at 18-20° C., and then allowed to stand for 30 minutes. The supernatant is removed to obtain modified nano zinc oxide.
[0033] Example 2
[0034] A modified nano zinc oxide comprises the following preparation steps:
[0035] After 12 mL of stearic acid and 30 mL of isopropanol were mixed and stirred evenly, 1.5 g of nano zinc oxide was added, and the mixture was stirred for 1.2 h at 18-20° C., and then allowed to stand for 40 min. The supernatant was removed to obtain modified nano zinc oxide.
[0036] Example 3
[0037] A wear-resistant coating comprises the following preparation steps:
[0038] The raw materials were weighed according to the formula, 9.4 g of deionized water, 1 g of silica sol, 1 g of sulfuryl chloride, and 5 g of the modified nano zinc oxide prepared in Example 1 were added into a reaction container, 10 g of mixed solution A (prepared by mixing 3-isocyanatepropyltriethoxysilane and methyl orthosilicate in a mass ratio of 5:1.3) was added dropwise, reacted at 80-85° C. for 30 min, cooled to 25±1.5° C., 2.8 g of silane coupling agent KH-560 and 14 g of isopropanol were added, and stirred for 1 h to obtain a wear-resistant coating.
[0039] Comparative Example 1
[0040] Compared with Example 3, this comparative example only replaces "5 g of modified nano zinc oxide prepared in Example 1" with "5 g of nano zinc oxide", and the remaining steps and parameters are the same.
[0041] Example 4
[0042] A wear-resistant coating comprises the following preparation steps:
[0043] The raw materials were weighed according to the formula, 15 g of deionized water, 8 g of silica sol, 1.2 g of sulfuryl chloride, and 8 g of the modified nano zinc oxide prepared in Example 2 were added into a reaction container, 14 g of mixed solution A (prepared by mixing 3-isocyanatepropyltriethoxysilane and methyl orthosilicate in a mass ratio of 6.5:1) was added dropwise, reacted at 80-85°C for 45 min, cooled to 25±1.5°C, 3.3 g of silane coupling agent KH-560 and 20 g of isopropanol were added, and stirred for 2 h to obtain a wear-resistant coating.
[0044] Example 5
[0045] A corrosion-resistant coating comprises the following preparation steps:
[0046] Step S1, dissolving 40g of epoxy resin E-44 in 40g of acetone, adding 20g of silicone resin TSR-144, 2g of silane coupling agent KH560, and 1g of dibutyltin dilaurate, heating to 80°C, reflux stirring for 1.5h, mixing thoroughly, cooling after reaction, and obtaining epoxy-modified silicone resin;
[0047] Step S2: 20 g of epoxy-modified silicone resin, 20 g of polytetrafluoroethylene powder and 20 g of defoamer BYK-141 are mixed and ground to a fineness of 25-30 μm, and then 1 g of curing agent T-31 is added and stirred evenly to obtain a corrosion-resistant coating.
[0048] Comparative Example 2
[0049] Compared with Example 5, this comparative example only does not add "20g of polytetrafluoroethylene powder", and the remaining steps and parameters are the same.
[0050] Example 6
[0051] A corrosion-resistant coating comprises the following preparation steps:
[0052] Step S1, dissolving 50g of epoxy resin E-44 in 50g of acetone, adding 30g of silicone resin TSR-144, 3g of silane coupling agent KH560, and 1.2g of dibutyltin dilaurate, heating to 90°C, reflux stirring for 2h, fully mixing, cooling after reaction, to obtain epoxy-modified silicone resin;
[0053] Step S2: 30 g of epoxy-modified silicone resin, 30 g of polytetrafluoroethylene powder and 30 g of defoamer BYK-141 are mixed and ground to a fineness of 25-30 μm, and then 5 g of curing agent T-31 is added and stirred evenly to obtain a corrosion-resistant coating.
[0054] Example 7
[0055] A method for preparing wear-resistant coated glass comprises the following preparation steps:
[0056] Step 1: Prepare a silicon nitride base layer on the surface of the glass body by using a DC magnetron sputtering technology (the target material is a silicon target, the functional gases are argon and nitrogen, the volume ratio of argon and nitrogen is 1:1, and the vacuum degree is 0.1 Pa);
[0057] Step 2: using a DC magnetron sputtering technique (the target material is a silver target) to prepare a silver-plated layer on the surface of the glass body;
[0058] Step 3, filter the wear-resistant coating prepared in Example 3 with a 3 μm microporous filter membrane, add a wetting and leveling agent BYK-333 (the mass ratio of the wear-resistant coating to the wetting and leveling agent BYK-333 is 100:0.3), mix, and apply it to the surface of the glass body by flow coating. After the surface is dry, dry it at a constant temperature of 40-50° C. for 1-2 hours to solidify the coating, and the wear-resistant layer is prepared;
[0059] Step 4: Spray the corrosion-resistant coating prepared in Example 5 onto the outside of the wear-resistant layer, and dry at 25±1.5°C for 24-30 hours to solidify the coating. The protective layer is prepared to obtain a wear-resistant coated glass.
[0060] Example 8
[0061] A method for preparing wear-resistant coated glass comprises the following preparation steps:
[0062] Step 1: Prepare a silicon nitride base layer on the surface of the glass body by using a DC magnetron sputtering technology (the target material is a silicon target, the functional gases are argon and nitrogen, the volume ratio of argon and nitrogen is 2:4.5, and the vacuum degree is 0.1 Pa);
[0063] Step 2: using a DC magnetron sputtering technique (the target material is a silver target) to prepare a silver-plated layer on the surface of the glass body;
[0064] Step 3: Filter the wear-resistant coating prepared in Example 4 with a 3 μm microporous filter membrane, add a wetting and leveling agent BYK-333 (the mass ratio of the wear-resistant coating to the wetting and leveling agent BYK-333 is 100:0.4), mix, and apply it to the surface of the glass body by flow coating. After the surface is dry, dry it at a constant temperature of 40-50° C. for 1-2 hours to solidify the coating, and the wear-resistant layer is prepared;
[0065] Step 4: Spray the corrosion-resistant coating prepared in Example 6 onto the outside of the wear-resistant layer, and dry at 25±1.5°C for 24-30 hours to solidify the coating. The protective layer is prepared to obtain a wear-resistant coated glass.
[0066] Example 9
[0067] A method for preparing wear-resistant coated glass comprises the following preparation steps:
[0068] Step 1: Prepare a silicon nitride base layer on the surface of the glass body by using a DC magnetron sputtering technology (the target material is a silicon target, the functional gases are argon and nitrogen, the volume ratio of argon and nitrogen is 3:8, and the vacuum degree is 1.33 Pa);
[0069] Step 2: using a DC magnetron sputtering technique (the target material is a silver target) to prepare a silver-plated layer on the surface of the glass body;
[0070] Step 3: Filter the wear-resistant coating prepared in Example 4 with a 3 μm microporous filter membrane, add a wetting and leveling agent BYK-333 (the mass ratio of the wear-resistant coating to the wetting and leveling agent BYK-333 is 100:0.35), mix, and apply it to the surface of the glass body by flow coating. After the surface is dry, dry it at a constant temperature of 40-50° C. for 1-2 hours to solidify the coating, and the wear-resistant layer is prepared;
[0071] Step 4: Spray the corrosion-resistant coating prepared in Example 5 on the outside of the wear-resistant layer, dry at 25±1.5°C for 24-30 hours to solidify the coating, and the protective layer is prepared to obtain a wear-resistant coated glass.
[0072] Comparative Example 3
[0073] Compared with Example 7, this comparative example only replaces the "wear-resistant coating prepared in Example 3" with the "wear-resistant coating prepared in Comparative Example 1", and the remaining steps and parameters are the same.
[0074] Comparative Example 4
[0075] Compared with Example 7, this comparative example only replaces the "corrosion-resistant coating prepared in Example 5" with the "corrosion-resistant coating prepared in Comparative Example 2", and the remaining steps and parameters are the same.
[0076] The following performance tests were performed on the coated glasses prepared in Examples 7-9 and Comparative Examples 3-4:
[0077] Light transmittance test: Use OU4220 visible / infrared / ultraviolet light transmittance meter to test the light transmittance of the coated glass to be tested, and record the measured data;
[0078] Abrasion resistance test: Test the abrasion resistance of the coated glass to be tested according to GB / T 18915.2-2013, and calculate the absolute value of the difference in visible light transmittance of the sample before and after the test;
[0079] Corrosion resistance test: According to GB / T 18915.2-2013, the acid resistance and alkali resistance of the coated glass to be tested are tested, and the absolute value of the difference in visible light transmittance of the sample before and after the test is calculated.
[0080] The test results are shown in Table 1.
[0081] Table 1
[0082]
[0083] It can be seen from Table 1 that the coated glasses prepared in Examples 7-9 have better light transmittance and wear resistance than the coated glass prepared in Comparative Example 3, and have better wear resistance and corrosion resistance than the coated glass prepared in Comparative Example 4.
[0084] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0085] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A wear-resistant coated glass, characterized in that: The invention comprises a glass body, wherein a silicon nitride primer layer, a silver-plated layer, a wear-resistant layer and a protective layer are sequentially arranged on the surface of the glass body; the material of the wear-resistant layer is a wear-resistant coating; the material of the protective layer is a corrosion-resistant coating; the wear-resistant coating comprises the following raw materials in parts by weight: 9.4-15 parts of deionized water, 1-8 parts of silica sol, 1-1.2 parts of sulfuryl chloride, 5-8 parts of modified nano zinc oxide, 10-14 parts of mixed solution A, 2.8-3.3 parts of silane coupling agent KH-560, and 14-20 parts of isopropyl alcohol; The modified nano zinc oxide comprises the following preparation steps: Mix 10-12 mL of stearic acid and 20-30 mL of isopropanol and stir evenly, then add 1-1.5 g of nano zinc oxide, continue stirring at 18-20°C for 1-1.2 hours, let stand for 30-40 minutes, remove the supernatant, and obtain modified nano zinc oxide; The mixed solution A is prepared by mixing 3-isocyanatepropyltriethoxysilane and methyl orthosilicate in a mass ratio of 5-6.5:1-1.3; The corrosion-resistant coating comprises the following preparation steps: Step S1, dissolving epoxy resin E-44 in acetone, adding silicone resin TSR-144, silane coupling agent KH560, and dibutyltin dilaurate, heating to 80-90° C., reflux stirring for 1.5-2 h, fully mixing, cooling after reaction, and obtaining epoxy-modified silicone resin; Step S2: After the epoxy-modified silicone resin, polytetrafluoroethylene powder and defoamer BYK-141 are mixed and ground to a fineness of 25-30 μm, curing agent T-31 is added and stirred evenly to obtain a corrosion-resistant coating.
2. The wear-resistant coated glass according to claim 1, characterized in that: The particle size of the silica sol is 12-15 nm.
3. The wear-resistant coated glass according to claim 1, characterized in that: The wear-resistant coating comprises the following preparation steps: Weigh the raw materials according to the formula, add deionized water, silica sol, sulfuryl chloride and modified nano zinc oxide into the reaction container, add mixed solution A dropwise, react at 80-85℃ for 30-45min, cool to 25±1.5℃, add silane coupling agent KH-560 and isopropanol, stir for 1-2h to obtain the wear-resistant coating.
4. The wear-resistant coated glass according to claim 1, characterized in that: In step S1, the mass ratio of the epoxy resin E-44, acetone, silicone resin TSR-144, silane coupling agent KH560, and dibutyltin dilaurate is 40-50:40-50:20-30:2-3:1-1.
2.
5. The wear-resistant coated glass according to claim 1, characterized in that: The mass ratio of the epoxy-modified silicone resin, polytetrafluoroethylene powder, defoamer BYK-141, and curing agent T-31 in step S2 is 20-30:20-30:20-30:1-5.
6. The method for preparing a wear-resistant coated glass according to claim 1, characterized in that: The method comprises the following preparation steps: Step 1: Prepare a silicon nitride base layer on the surface of the glass body by using a DC magnetron sputtering technique; Step 2: preparing a silver-plated layer on the surface of the glass body by using a DC magnetron sputtering technique; Step 3: Filter the wear-resistant coating with a 3 μm microporous filter membrane, add the wetting and leveling agent BYK-333 and mix, apply it on the surface of the silver-plated layer by flow coating, and after the surface is dry, dry it at a constant temperature of 40-50° C. for 1-2 hours to complete the preparation of the wear-resistant layer; Step 4: Spray the corrosion-resistant coating on the outside of the wear-resistant layer, dry at 25±1.5°C for 24-30 hours, and the protective layer is prepared to obtain a wear-resistant coated glass.
7. The method for preparing a wear-resistant coated glass according to claim 6, characterized in that: The mass ratio of the wear-resistant coating to the wetting and leveling agent BYK-333 is 100:0.3-0.4.