A broadband absorbing electrochromic polymer and a preparation method thereof, and an electrochromic film
Patent Information
- Application Number
- CN202211490004.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-25
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-11-25
AI Technical Summary
而目前,也尚未见相关聚合物的报道
[0021]由于在4,9-二氢-s-苯并二茚并[1,2-B:5,6-b']二噻吩(IDT)主链内嵌入4,7-二溴-2,1,3-苯并噻二唑(TZ)、2,5-二溴-3,4-乙撑二氧噻吩(Br-EDOT)和苯并噻二唑并[3,4-g]喹喔啉(TQX)单元,使得本发明宽波段吸收的电致变色聚合物和包含它的电致变色薄膜表现出广泛的光谱吸收行为,可显示黑褐色至透明色的变换,且具有高对比度、快响应速率和高稳定性,可应用于电致变色器件中。
Smart Images

Figure CN115926119B_ABST
Abstract
Description
Technical Field
[0001] The present invention generally relates to the field of electrochromic technology, and in particular to an electrochromic polymer with wide-band absorption, a preparation method thereof, and an electrochromic polymer film. Background Art
[0002] Electrochromic materials refer to materials whose optical properties change due to a reversible redox reaction under the action of an external electric field. They have broad application prospects in the fields of smart windows, anti-glare rearview mirrors, and military intelligent camouflage. Generally, electrochromic materials include transition metal oxides, viologens, small molecules, conductive polymers, etc. Among them, conductive polymers have become a hot spot in the current research and application of electrochromic materials due to their advantages such as designable structure, rich color changes, high contrast, fast response rate, high coloring efficiency, and good stability. However, there are few reports on polymers with wide-band absorption. Therefore, the development of black polymers with broad spectral absorption is of great significance to the field of electrochromism.
[0003] Designing donor-acceptor polymer structures is an effective means to achieve wide-spectrum absorption. First, the acceptor structure is designed to red-shift the absorption spectrum of the polymer by regulating the intramolecular charge transfer effect directly related to long-wave absorption; second, the donor unit in the polymer is designed to optimize its short-wave color-changing performance by regulating the π-π* transition effect directly related to short-wave absorption; finally, according to the optical compensation mechanism, characteristic optical and near-infrared absorption units are introduced into the polymer main chain for the absorption trough to achieve the effect of wide-band absorption.
[0004] In recent years, 4,9-dihydro-s-indolo[1,2-b:5,6-b0]dithiophene (IDT) has been increasingly used as a main building block for conjugated polymer electronic materials. 3 The availability of hybridized carbon atoms allows functional side chains to be easily attached to the IDT unit to increase its solubility. In addition, the inherent coplanar "ladder" structure of the IDT unit enhances the degree of π electron delocalization, making it highly electron-rich and having good electron-donating ability. Benzothiadiazole [3,4-g] quinoxaline (TQX) is used as an acceptor unit. The C=N double bond in the conjugated ring can effectively enhance the electron-withdrawing ability while maintaining the good planarity of the conjugated structure. In addition, TQX has less steric hindrance when combined with donors such as thiophene, which can ensure that the polymer absorption spectrum is in the near-infrared region. At the same time, the introduction of 4,7-dibromo-2,1,3-benzothiadiazole (TZ) and 2,5-dibromo-3,4-ethylenedioxythiophene (Br-EDOT) well compensates for the valley area of the visible light band, thereby effectively achieving a wide range of spectral absorption. At present, there is no report on related polymers. Summary of the invention
[0005] The purpose of the present invention is to design and prepare an electrochromic polymer with wide-band absorption and an electrochromic film comprising the electrochromic polymer. The electrochromic polymer structure contains 4,9-dihydro-s-indoxybenzo[1,2-B:5,6-b']dithiophene (IDT), 4,7-dibromo-2,1,3-benzothiadiazole (TZ), 2,5-dibromo-3,4-ethylenedioxythiophene (Br-EDOT) and benzothiadiazole[3,4-g]quinoxaline (TQX) units. The polymer film of the electrochromic copolymer is prepared by a Stille coupling method to synthesize two new random quaternary conjugated polymers.
[0006] The technical solution of the present invention is to first provide an electrochromic polymer with wide-band absorption, including a compound shown in the following structural formula:
[0007]
[0008] Wherein, R1 is a straight-chain alkyl group with more than 6 carbon atoms, R2 is a branched-chain alkyl group with more than 20 carbon atoms, m and n both represent the degree of polymerization, and the values of m and n are each independently a natural number between 8 and 100.
[0009] The compound shown in the structural formula includes 4,9-dihydro-s-benzoindano[1,2-B:5,6-b']dithiophene (IDT), 4,7-dibromo-2,1,3-benzothiadiazole (TZ), 2,5-dibromo-3,4-ethylenedioxythiophene (Br-EDOT) and benzothiadiazole[3,4-g]quinoxaline (TQX) units.
[0010] The present invention also provides a method for preparing the above-mentioned electrochromic polymer with wide-band absorption, comprising the following steps:
[0011] 1) Preparation of polymer by Stille coupling: 4,9-dihydro-s-benzoindo[1,2-B:5,6-b']dithiophene (M1), 2,5-dibromo-3,4-ethylenedioxythiophene (M2), 4,7-dibromo-2,1,3-benzothiadiazole (M3), benzothiadiazole[3,4-g]quinoxaline (M4), xylene, tris(dibenzylideneacetone)dipalladium and tris(2-methylphenyl)phosphine were added into a two-necked flask with an atmosphere protection and a condenser on top, and the flask was vented to maintain the atmosphere protection in the flask. The mixture was heated for reaction and then cooled to room temperature, the reaction solution was dropped into methanol for precipitation, and the dark brown precipitate was collected by filtration;
[0012] 2) Purify the polymer by Soxhlet extraction: Wrap the dark brown precipitate with filter paper, place it in a fat extractor, wash it with methanol, n-hexane and chloroform in sequence, concentrate the chloroform washing liquid, drop it into methanol for precipitation, and filter and collect the precipitate to obtain the purified electrochromic polymer.
[0013] The synthetic route is as follows:
[0014]
[0015] Wherein, R1 is a straight-chain alkyl group with more than 6 carbon atoms, R2 is a branched-chain alkyl group with more than 20 carbon atoms, m and n both represent the degree of polymerization, and the values of m and n are each independently a natural number between 8 and 100.
[0016] Furthermore, in the above step 1), the molar ratio of M1:M3 is (8:1)-(3:1), the molar ratio of M1:M3 is (4:1)-(3:1), and the molar ratio of M1:M4 is (3:1)-(2.5:1).
[0017] Furthermore, in the above step 1), the molar ratio of 4,9-dihydro-s-benzoindo[1,2-B:5,6-b']dithiophene (M1) to tri(dibenzylideneacetone)dipalladium is 1:(0.02-0.04); the molar ratio of 4,9-dihydro-s-benzoindo[1,2-B:5,6-b']dithiophene (M1) to tri(2-methylphenyl)phosphine is 1:(0.1-0.2); and the amount of xylene used is such that the concentration of each monomer is 0.3 mol / L.
[0018] Furthermore, the reaction temperature in the above step 1) is 100-120° C., and the reaction time is 48-96 hours.
[0019] Furthermore, the purification process in the above step 2) is a Soxhlet extraction process, in which methanol, n-hexane and chloroform are used for extraction in sequence, and the chloroform solution is precipitated.
[0020] The present invention also provides an electrochromic film, which is obtained by spraying or scraping the electrochromic polymer with wide-band absorption provided by the present invention, and the film thickness of the film is 200-800nm. The electrochromic polymer with wide-band absorption can be formed on the surface of a conductive substrate by scraping and spraying a solution, and its color switches between dark brown and transparent states, and has the characteristics of low driving voltage, high optical contrast, and high stability, and is suitable for assembly and application of electrochromic devices.
[0021] Since 4,7-dibromo-2,1,3-benzothiadiazole (TZ), 2,5-dibromo-3,4-ethylenedioxythiophene (Br-EDOT) and benzothiadiazole [3,4-g] quinoxaline (TQX) units are embedded in the main chain of 4,9-dihydro-s-indano[1,2-B:5,6-b']dithiophene (IDT), the electrochromic polymer with wide-band absorption and the electrochromic film containing the same of the present invention exhibit a wide range of spectral absorption behavior, can show a change from dark brown to transparent color, and have high contrast, fast response rate and high stability, and can be applied to electrochromic devices.
[0022] The present invention uses 4,9-dihydro-s-benzoindano[1,2-B:5,6-b']dithiophene (IDT), 4,7-dibromo-2,1,3-benzothiadiazole (TZ), 2,5-dibromo-3,4-ethylenedioxythiophene (Br-EDOT) and benzothiadiazole[3,4-g]quinoxaline (TQX) as monomers to design and synthesize two new types of random quaternary conjugated polymers. The polymer spectral absorption principle is used to achieve the preparation of electrochromic polymers with wide spectral absorption. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] These and / or other aspects and advantages of the present invention will become more clear and easier to understand from the following detailed description of the embodiments of the present invention in conjunction with the accompanying drawings, in which:
[0024] Figure 1 This is the H NMR spectrum of the target polymer IDT-EDOT-TZ-TQX-3-1-1-1 obtained in the example of the present invention;
[0025] Figure 2 This is the H NMR spectrum of the target polymer IDT-EDOT-TZ-TQX-4-0.5-1-2.5 obtained in the example of the present invention;
[0026] Figure 3 The spectral absorption curve and color photograph of the polymer obtained in the embodiment of the present invention dissolved in chloroform;
[0027] Figure 4 The UV-visible absorption spectra and color change photos of the copolymer film obtained in the embodiment of the present invention at different potentials;
[0028] Figure 5 The electrochemical cyclic voltammetry curve of the copolymer film obtained in the embodiment of the present invention;
[0029] Figure 6 The chronograph transmittance response and stability curve of the copolymer film obtained in the embodiment of the present invention;
[0030] Figure 7This is the thermal stability curve of the copolymer obtained in the example of the present invention. DETAILED DESCRIPTION
[0031] In order to enable those skilled in the art to better understand the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and specific implementation methods.
[0032] Example 1
[0033] A method for preparing a broadband absorbing electrochromic polymer comprises the following steps:
[0034] (1) Synthesis of 2,5-dibromo-3,4-ethylenedioxythiophene (Br-EDOT)
[0035] Dissolve 0.1 mol of 3,4-ethylenedioxythiophene in 20 mL of chloroform and place it in a 100 mL two-necked bottle. Protect the two-necked bottle with argon and cover it with tin foil to avoid light. Dissolve 0.3 mmol of NBS (N-bromosuccinimide) in 10 mL of N,N-dimethylformamide (DMF) and slowly inject it into the reaction bottle through a syringe. Stir and react for 36 hours. Pour the reaction solution into water, separate and collect the organic phase, extract the aqueous phase twice with 20 mL of dichloromethane, combine the organic phases, dry with anhydrous magnesium sulfate, pass through a silica gel column, and use dichloromethane / n-hexane (2:1) as the eluent. Rotary evaporation gives a silvery white crystalline solid. This intermediate product is unstable. In order to avoid spontaneous polymerization, the subsequent steps of the synthesis must be carried out within 24 hours after the solid product is separated. The hydrogen nuclear magnetic resonance spectrum of the compound prepared in this step 1 HNMR (400MHz, CDCl3, δ, ppm): 4.27 (s, 4H).
[0036] (2) Synthesis of benzothiadiazo[3,4-g]quinoxaline (TQX)
[0037] 4,7-dibromobenzo[C][1,2,5]thiadiazole-5,6-diamine (1g, 3mmol), product 1,2-bis(4-(decyloxy)phenyl)ethane-1,2-dione (1.5g, 2.8mmol) and 40ml glacial acetic acid were added to a 100ml round-bottom flask, the reaction mixture was refluxed overnight, the reactant was cooled to room temperature, poured into 100ml deionized water, extracted with dichloromethane, dried with anhydrous magnesium sulfate, and purified by column chromatography to obtain an orange-red solid. The yield was 80%; the corresponding H NMR spectrum 1 H NMR (400MHz, CDCl3): 7.96-7.80 (d, 4H), 6.98-6.95 (d, 4H), 3.90 (d, 4H), 1.81 (sep, 2H), 1.29 (m, 64H), 0.90 (m, 12H). 13C NMR (101MHz, CDCl3): δ161.47,155.74,138.07,132.64,131.88,71.14,38.10,31.93,31.27,30.04,26.88,22.71,14.30.
[0038] (3) Synthesis of electrochromic polymers with broad-band absorption
[0039] 1. Place 0.3 mmol of 4,9-dihydro-s-benzoindano[1,2-B:5,6-b']dithiophene (IDT), 0.1 mmol of 4,7-dibromo-2,1,3-benzothiadiazole (TZ), 0.1 mmol of 2,5-dibromo-3,4-ethylenedioxythiophene (Br-EDOT), 0.1 mmol of benzothiadiazole[3,4-g]quinoxaline (TQX), 0.006 mmol of tris(dibenzylideneacetone)dipalladium, and 0.03 mmol of tris(2-methylphenyl)phosphine in a 25 mL two-necked bottle, evacuate and inject nitrogen, inject 15 mL of anhydrous xylene, and evacuate again. The reaction mixture was filled with nitrogen and heated to 120°C for reflux reaction for 72 hours. After the reaction was completed, it was cooled to room temperature and the reaction solution was dropped into cold methanol for precipitation. The precipitate was filtered and dried. Soxhlet extraction was performed with methanol, n-hexane and chloroform respectively, and the extraction time for each time was 24 hours. The chloroform extract was concentrated to 15 mL and then dropped into cold methanol for precipitation to obtain a black solid. The target polymer IDT-EDOT-TZ-TQX-3-1-1-1 (the 3-1-1-1 in the target polymer expression formula indicates that the molar ratio of IDT: Br-EDOT: TZ: TQX in the raw material is 3:1:1:1) was obtained by filtration and drying with a yield of 60%.
[0040] 2. Place 0.4 mmol of 4,9-dihydro-s-benzoindano[1,2-B:5,6-b']dithiophene (IDT), 0.05 mmol of 4,7-dibromo-2,1,3-benzothiadiazole (TZ), 0.1 mmol of 2,5-dibromo-3,4-ethylenedioxythiophene (Br-EDOT), 0.2 mmol of benzothiadiazole[3,4-g]quinoxaline (TQX), 0.008 mmol of tris(dibenzylideneacetone)dipalladium, and 0.04 mmol of tris(2-methylphenyl)phosphine in a 25 mL two-necked bottle, ventilate, inject nitrogen, inject 15 mL of anhydrous xylene, and ventilate again. The mixture was ventilated and filled with nitrogen, heated to 120°C and refluxed for 72 hours. After the reaction was completed, the mixture was cooled to room temperature, and the reaction solution was dropped into cold methanol for precipitation. The precipitate was filtered and dried. Then, Soxhlet extraction was performed with methanol, n-hexane and chloroform, respectively. The extraction time for each time was 24 hours. The chloroform extract was concentrated to 15 mL, and then dropped into cold methanol for precipitation to obtain a black solid. The target polymer IDT-EDOT-TZ-TQX-4-0.5-1-2.5 was obtained after filtration and drying (the 4-0.5-1-2.5 in the target polymer expression formula indicates that the molar ratio of IDT: Br-EDOT: TZ: TQX in the raw material is 4:0.5:1:
[0041] 2.5), with a yield of 66%.
[0042] The H NMR spectra of all copolymers are shown in Figure 1 and Figure 2 .
[0043] Example 2
[0044] The polymer prepared in Example 1 was subjected to solution spectrum and electrochemical performance tests. The polymer was dissolved in chloroform to a concentration of 2*10 -4 mg / mL solution, the solution absorption curve and photo are as follows Figure 3 As shown, the polymer solutions are all dark brown. Through the test of UV-visible spectrophotometer, the solutions of both polymers have a relatively wide absorption band and show several high absorption peaks, which are the result of the combined action of π electron transition and intramolecular charge transfer. Among them, the absorption peaks corresponding to the polymer IDT-EDOT-TZ-TQX-3-1-1-1 are at 516nm, 564nm and 842nm respectively. The absorption peaks corresponding to the polymer IDT-EDOT-TZ-TQX-4-0.5-1-2.5 are at 452nm, 561nm and 871nm respectively.
[0045] Preparation of polymer film: dissolve the polymer in chloroform to prepare a 5mg / ml solution, filter out the insoluble matter through a filter, place it in a spray gun, control the air pressure to 2MPa, spray it on the conductive glass, the film absorbance is about 1.0, and place it in a vacuum drying oven at 40 degrees for vacuum drying. A three-electrode system with a polymer film as the working electrode, a platinum wire as the counter electrode, and a calibrated silver wire as the reference electrode is used, and the supporting electrolyte is: 0.1mol / L lithium perchlorate propylene carbonate solution.
[0046] The copolymer film was tested for spectroelectrochemical performance under different voltages. A three-electrode system was used, with platinum wire as the counter electrode, calibrated silver wire as the reference electrode, polymer film as the working electrode, and the supporting electrolyte being 0.1 mol / L lithium perchlorate propylene carbonate solution. The spectroelectrochemical spectra and color-decolorized photos of the two copolymer films under different applied voltages are shown in Figure 4 , indicating that the copolymer films all have obvious electrochromic properties. Due to the accumulation of π-π* bonds, the spectrum of the polymer film has a certain red shift relative to the solution. As the voltage continues to increase, the polymer film can achieve a transition from a neutral state to a transparent state.
[0047] The electrochemical properties of the copolymers were tested by cyclic voltammetry (see Figure 5 ), both polymers have low oxidation potentials. The initial oxidation potential of IDT-EDOT-TZ-TQX-3-1-1-1 is 0.46V, and the initial oxidation potential of IDT-EDOT-TZ-TQX-4-0.5-1-2.5 is 0.45V. Both have reversible redox activity, accompanied by reversible color changes.
[0048] The response time refers to the time required for the material to achieve a 95% difference in its maximum transmittance. The response time and cycle stability of the polymer were tested using a UV-visible spectrophotometer and an electrochemical workstation (see Figure 6 ), connect the three-electrode system to the electrochemical workstation, and place the quartz cuvette in the UV-visible spectrophotometer. While applying voltage to the polymer film, simultaneously measure the change in transmittance at the wavelength of maximum transmittance. It takes 8.6 seconds for the transmittance of DT-EDOT-TZ-TQX-3-1-1-1 at 521nm to change from 4.7% before oxidation to 43.8%, while the reduction process is relatively fast, and it takes 4.5 seconds to drop from 47.9% to 11.2%. It takes 15 seconds for the transmittance of IDT-EDOT-TZ-TQX-4-0.5-1-2.5 at 489nm to change from 6.7% before oxidation to 47.3%, and only 5 seconds to drop from 51.8% to 11.3%. And after multiple cycles, there is no obvious attenuation of contrast.
[0049] Testing the thermal stability of electrochromic polymers (see Figure 7 ): The thermal decomposition temperature of the polymer is greater than 300°C, indicating that it can be used in a working environment with higher temperatures.
[0050] It can be seen from the above embodiments that the color and absorption spectrum of the copolymer film prepared by the present invention can be regulated by the type of copolymer monomers, the copolymer film can achieve a transformation from colored to transparent, and has the characteristics of low driving potential, high coloring efficiency, good stability, etc. The prepared copolymer film can be used in the fields of electrochromic display, adaptive camouflage, etc.
[0051] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and variations will be apparent to those of ordinary skill in the art without departing from the scope and spirit of the described embodiments. Therefore, the scope of protection of the present invention should be subject to the scope of protection of the claims.
Claims
1. A broadband absorbing electrochromic polymer, characterized in that: Including compounds shown in the following structural formula: Wherein, R1 is a straight-chain alkyl group with more than 6 carbon atoms, R2 is a branched-chain alkyl group with more than 20 carbon atoms, m and n both represent the degree of polymerization, and the values of m and n are each independently a natural number between 8 and 100.
2. The method for preparing a broadband absorbing electrochromic polymer according to claim 1, characterized in that: The following steps are involved: 1) Preparation of polymer by Stille coupling: 4,9-dihydro-s-benzoindo[1,2-B:5,6-b']dithiophene (M1), 2,5-dibromo-3,4-ethylenedioxythiophene (M2), 4,7-dibromo-2,1,3-benzothiadiazole (M3), benzothiadiazole[3,4-g]quinoxaline (M4), xylene, tris(dibenzylideneacetone)dipalladium and tris(2-methylphenyl)phosphine were added into a two-necked flask with an atmosphere protection and a condenser on top, and the flask was vented to maintain the atmosphere protection in the flask. The mixture was heated for reaction and then cooled to room temperature, the reaction solution was dropped into methanol for precipitation, and the dark brown precipitate was collected by filtration; The structural formula of the 4,9-dihydro-s-benzoindene[1,2-B:5,6-b']dithiophene (M1) is as follows: The structural formula of the benzothiadiazole [3,4-g] quinoxaline (M4) is as follows: 2) Purify the polymer by Soxhlet extraction: Wrap the dark brown precipitate with filter paper, place it in a fat extractor, wash it with methanol, n-hexane and chloroform in sequence, concentrate the chloroform washing liquid, drop it into methanol for precipitation, and filter and collect the precipitate to obtain the purified electrochromic polymer.
3. The method for preparing the electrochromic polymer with broadband absorption as claimed in claim 2, characterized in that: In the step 1), the molar ratio of 4,9-dihydro-s-indan[1,2-B:5,6-b']dithiophene (M1) to 2,5-dibromo-3,4-ethylenedioxythiophene (M2) is (8:1)-(3:1), the molar ratio of 4,9-dihydro-s-indan[1,2-B:5,6-b']dithiophene (M1) to 4,7-dibromo-2,1,3-benzothiadiazole (M3) is (4:1)-(3:1), and the molar ratio of 4,9-dihydro-s-indan[1,2-B:5,6-b']dithiophene (M1) to benzothiadiazole[3,4-g]quinoxaline (M4) is (3:1)-(2.5:1).
4. The method for preparing a broadband absorbing electrochromic polymer according to claim 2, characterized in that: In the step 1): The molar ratio of 4,9-dihydro-s-benzoindeno[1,2-B:5,6-b']dithiophene (M1) to tris(dibenzylideneacetone)dipalladium is 1:(0.02-0.04); The molar ratio of 4,9-dihydro-s-benzoindo[1,2-B:5,6-b']dithiophene (M1) to tri(2-methylphenyl)phosphine is 1:(0.1-0.2); the amount of xylene used is such that the concentration of each monomer is 0.3 mol / L.
5. The method for preparing a broadband absorbing electrochromic polymer according to claim 2, characterized in that: The reaction temperature in step 1) is 100-120° C., and the reaction time is 48-96 hours.
6. The method for preparing a broadband absorbing electrochromic polymer according to claim 2, characterized in that: The purification process in step 2) is a Soxhlet extraction process, in which methanol, n-hexane and chloroform are used in sequence for extraction, and the chloroform solution is precipitated.
7. An electrochromic film, characterized in that: The film is obtained by spraying or scraping the electrochromic polymer with wide-band absorption as claimed in claim 1, and the film thickness of the film is 200-800 nm.
Citation Information
Patent Citations
Active materials for photoelectric devices
CN102164926A
Green polythiophenes electrochromic material and preparation method thereof as well as component
CN103772664A
Tetra-aryl indacenodithiophene-based polycyclic polymers and their use
CN106459386A
Electrochromic polymer containing indacenodithiophene structure, preparation method, polymer film and application
CN112430314A
Method for Preparing Dioxyheterocycle-Based Electrochromic Polymers
US20160122476A1