Molding material for waterproof and breathable flower pot and preparation method thereof

By using a molding compound preparation method with components such as pre-treated resin clay mixture and unsaturated polyester resin in the flower pot material, the problems of poor waterproof and breathable performance and insufficient strength of the flower pot material are solved, and a more suitable plant growth environment is achieved. and improved material durability.

CN115926412BActive Publication Date: 2024-10-29江苏常阳科技有限公司
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211735950.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-30
Publication Date
2024-10-29
Estimated Expiration
2042-12-30

AI Technical Summary

Technical Problem

Existing flower pot materials have problems such as poor waterproof and breathable performance, insufficient strength, and poor durability, which limits the difference between the growing environment of plants and normal soil. Moreover, they are expensive and are not conducive to large-scale promotion.

Method used

A molding compound including pretreated resin clay mixture, unsaturated polyester resin, fillers, initiators, rheology regulators, additives and reinforcing fibers is used. Through premixing of high solid content resin and clay, vacuum drying, resin The paste is dispersed and mixed to form a molding compound with a porous structure, which improves waterproof and breathable performance and strength.

Benefits of technology

It significantly improves the waterproof and breathable performance and strength of the flowerpot material, simulates the growth environment of plants in the soil, reduces the requirements for plant survival soil, and improves the material's fall resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004032453060000061
    Figure BDA0004032453060000061
  • Figure BDA0004032453060000071
    Figure BDA0004032453060000071
Patent Text Reader

Abstract

The present invention provides a molding material for waterproof and breathable flower pots, comprising the following components in mass percentage: 15-50% pre-treated resin-clay mixture, 9-20% matrix resin, 20-75% filler, 0.5-1.5% initiator, 0.1-1% rheology regulator, 0.5-3% auxiliary agent and 0-30% reinforcing fiber; the pre-treated resin-clay mixture is obtained by mixing high-solid content resin with clay and then vacuum drying to form a pre-treated resin-clay mixture with a porous structure; the high-solid content resin has a resin solid content greater than 80%, the mass ratio of the high-solid content resin to the clay is 1:2-1:1, and the mass of the clay is not less than 10% of the total mass of the molding material. The present invention obtains a pre-treated resin-clay mixture with a porous structure by pre-mixing the high-solid content resin with clay, vacuum drying, and then mixing and dispersing the matrix resin with the initiator, rheology regulator, auxiliary agent and reinforcing fiber to obtain a molding material with good waterproof and breathable properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a molding compound for a waterproof and breathable flower pot and a preparation method of the molding compound, belonging to the technical field of resin materials. Background Art

[0002] With the progress of society and the improvement of people's living standards, the cultivation of flowers and plants is becoming more and more popular. At the same time, due to the continuous improvement of production conditions, the idea of ​​relying entirely on land for cultivation is no longer applicable to today's society. The use of fixed containers and soil for planting can better cope with the changing climate and provide plants with a suitable environment. Therefore, it will be vigorously promoted in the near future. Therefore, the demand for flower pots is gradually increasing.

[0003] Existing flower pot materials often have some problems. For example, ceramic flower pots are brittle and not resistant to falling, and plastic flower pots are not strong enough, and have poor weather resistance, durability, and corrosion resistance. In addition, there is an obvious disadvantage that the flower pot material is not breathable, which leads to a large difference between the growth environment of plants and the growth environment in normal soil, and the growth of plants is restricted. Current high-end flower pots, such as purple clay flower pots, can only partially meet the requirements of waterproof and breathable flower pots. They are brittle and easy to break, and are expensive, which is not conducive to large-scale promotion. In view of these problems, it is crucial to develop a material with low price, excellent comprehensive performance, especially waterproof and breathable properties. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a molding compound for a waterproof and breathable flower pot with good waterproof and breathable properties, high strength and good toughness, and a preparation method of the molding compound.

[0005] The present invention provides a technical solution to solve the above technical problems: a molding material for waterproof and breathable flower pots, comprising the following components in percentage by mass: 15-50% of a pretreated resin-clay mixture, 9-20% of a matrix resin, 20-75% of a filler, 0.5-1.5% of an initiator, 0.1-1% of a rheology regulator, 0.5-3% of an auxiliary agent and 0-30% of a reinforcing fiber; the pretreated resin-clay mixture is prepared by mixing a high-solid content resin with clay and then vacuum drying to form a pretreated resin-clay mixture with a porous structure; the high-solid content resin has a resin solid content greater than 80%, the mass ratio of the high-solid content resin to the clay is 1:2-1:1, and the mass of the clay is not less than 10% of the total mass of the molding material.

[0006] Furthermore, the clay is one or more of purple clay, red clay, white clay, and yellow clay. The particle size of the clay is 5 to 425 μm, and the clay is commercially available.

[0007] Furthermore, the high solid content resin and the matrix resin are unsaturated polyester resin or vinyl resin; and the filler is one or more of calcium carbonate, aluminum hydroxide and barium sulfate.

[0008] Furthermore, the high-solid content resin and the matrix resin contain unsaturated cross-linking monomers; the unsaturated cross-linking monomers are one or more of styrene, vinyl toluene, α-methylstyrene, vinyl chloride benzene, divinyl benzene, diallyl phthalate and methyl methacrylate; the mass of the unsaturated cross-linking monomers in the high-solid content resin is not more than 20% of the total mass of the high-solid content resin, and the mass of the unsaturated cross-linking monomers in the matrix resin accounts for 30-50% of the total mass of the matrix resin; the filler contains one or more of graphite, carbon black, carbon nanotubes, graphene, elemental silicon powder, silicon dioxide powder, mica, fly ash and glass beads.

[0009] Further, the initiator is one or more of tert-butyl perbenzoate, diacetyl peroxide, dibenzoyl peroxide, peroxyoctanoate and tert-butyl perbenzoate;

[0010] Furthermore, the rheology modifier is an alkaline earth metal oxide (such as MgO, CaO) and an alkaline earth metal hydroxide (such as Mg(OH) 2 ,Ga(OH) 2 ), one or more of carbodiamide, aziridine, polyisocyanate, polytetrafluoroethylene, perfluoropolyether, polyethylene, clay, and pyrogenic silica;

[0011] The auxiliary agent is one or more of a release agent, a dispersant, a viscosity reducer, and a defoaming agent.

[0012] Furthermore, the content of the release agent is 0.5-3% of the total amount, such as calcium stearate, zinc stearate, for example, calcium stearate produced by Dongguan Hanwei Technology Co., Ltd. Other additives include one or more of dispersants, viscosity reducers, and defoamers, and the content of other additives is 0-5% of the total amount.

[0013] Furthermore, the reinforcing fibers include one or more mixtures of glass fibers, carbon fibers, and aramid fibers.

[0014] Further, the fiber length may be selected to be 3-12 mm, more preferably, the fiber length may be selected to be 3-6 mm, for example, Owens' ECS979-14 6 mm glass fiber may be selected.

[0015] Furthermore, the matrix resin contains thermoplastic resin.

[0016] In order to solve the above technical problems, the present invention also provides a method for preparing the above-mentioned molding material for waterproof and breathable flower pots, comprising the following steps:

[0017] A. Premixing a high solid content resin and clay, placing the obtained premix in a vacuum drying oven at a temperature of 50° C. to 60° C., a vacuum degree of 0.2 to 0.6 MPa, and a vacuum drying time of 2 to 6 hours to form a pretreated resin-clay mixture having a porous structure;

[0018] B. mixing the base resin, initiator, rheology modifier and additives, and dispersing them using a high-speed disperser to obtain a resin paste;

[0019] C. After mixing the resin paste, filler and reinforcing fiber, add the pretreated resin clay mixture and continue mixing to obtain a molding compound.

[0020] Furthermore, the rotation speed of the first mixing is 1000-1500 rpm, and the dispersion time is at least 10 minutes.

[0021] Furthermore, in the step C, the resin paste, filler and reinforcing fiber are first mixed for 15 to 30 minutes, and then the pretreated resin clay mixture is added and mixed for 2 to 5 minutes.

[0022] The present invention has positive effects: the present invention provides a molding compound for waterproof and breathable flower pots and a preparation method thereof, wherein clay and a second filler are uniformly mixed and filled in the system, and a resin material is used as an adhesive, and the waterproof and breathable performance thereof is greatly improved compared with the existing flower pot materials, and the living environment of plants in the land can be effectively simulated, which is more suitable for plant growth and can reduce the requirements for plant living soil. At the same time, the existing flower pot products often have the disadvantages of low material strength and poor resistance to falling, while the flower pot material made of the bulk molding compound has higher strength, and the toughness is also greatly improved compared with the ceramic material, and is more resistant to falling. DETAILED DESCRIPTION

[0023] Example 1

[0024] The method for preparing the molding material for the waterproof and breathable flower pot of this embodiment comprises the following steps:

[0025] A. 80 parts of a base resin with a low styrene content and 150 parts of purple clay are pre-mixed and mixed using an open mill to form a state where no individual powder falls but no excess resin, i.e., a pre-mixture; the mixed material is placed in a vacuum drying oven at 50° C., the vacuum degree is 0.4 MPa, the vacuum drying time is 5 hours, and the system is evacuated to form a porous mixture;

[0026] B. 100 parts of the base resin are mixed with 10 parts of the initiator TBPB, 1 part of the rheology modifier MgO, and 15 parts of the release agent calcium stearate, and dispersed using a high-speed disperser with an adjustable speed of 1000 rpm for 15 minutes to prepare a resin paste for molding material;

[0027] C. Use a mixing machine to fully mix the resin paste, 450 parts of filler calcium carbonate, and 100 parts of glass fiber. The mixing machine includes one of a kneader, a three-roll grinder, an open mixer, and an internal mixer. The mixing time is 20 minutes. Add the mixed materials while stirring. Mix for 5 minutes. Package after mixing.

[0028] Example 2

[0029] The method for preparing the molding material for the waterproof and breathable flower pot of this embodiment comprises the following steps:

[0030] A. Premix 100 parts of a base resin with a low styrene content with 200 parts of purple clay, and mix them using an open mill to form a state where no separate powder falls but no excess resin, i.e., a premix; place the mixed material in a vacuum drying oven at 50°C, with a vacuum degree of 0.5Mpa, and a vacuum drying time of 4 hours, and evacuate the system to form pores;

[0031] B. 80 parts of the base resin are mixed with 10 parts of the initiator TBPB, 1 part of the rheology modifier MgO, and 15 parts of the release agent calcium stearate, and dispersed using a high-speed disperser with an adjustable speed of 1000 rpm for 15 minutes to prepare a resin paste for molding material;

[0032] C. Use resin paste, 300 parts of calcium carbonate filler, and 100 parts of glass fiber to mix thoroughly for 20 minutes, add the mixed materials, add while stirring, mix for 5 minutes, and package after mixing.

[0033] Example 3

[0034] The method for preparing the molding material for the waterproof and breathable flower pot of this embodiment comprises the following steps:

[0035] A. Premix 100 parts of a base resin with a low styrene content with 100 parts of purple clay, and mix them using an open mill to form a state where no individual powder falls but no excess resin, i.e., a premix; place the mixed material in a vacuum drying oven at 60° C., with a vacuum degree of 0.6 MPa, and a vacuum drying time of 4 hours, and evacuate the system to form pores;

[0036] B. 100 parts of the base resin are mixed with 10 parts of the initiator TBPB, 1 part of the rheology modifier MgO, and 15 parts of the release agent calcium stearate, and dispersed using a high-speed disperser with an adjustable speed of 1000 rpm for 15 minutes to prepare a resin paste for molding material;

[0037] C. Use resin paste and 600 parts of filler calcium carbonate to mix thoroughly for 20 minutes, add the mixed materials, add while stirring, mix for 5 minutes, and package after mixing.

[0038] Example 4

[0039] The method for preparing the molding material for the waterproof and breathable flower pot of this embodiment comprises the following steps:

[0040] A. Premix 200 parts of a base resin with a low styrene content with 300 parts of purple clay, and mix them using an open mill to form a state where no individual powder falls but no excess resin, i.e., a premix; place the mixed material in a vacuum drying oven at 55°C, with a vacuum degree of 0.3Mpa, and a vacuum drying time of 6 hours, and evacuate the system to form pores;

[0041] B. 180 parts of the base resin are mixed with 5 parts of the initiator TBPB, 8 parts of the rheology modifier carbon diamide MgO, and 5 parts of the release agent calcium stearate, and dispersed using a high-speed disperser with an adjustable speed of 1000 rpm for 15 minutes to prepare a resin paste for molding material;

[0042] C. Use resin paste, 3 parts of filler silica powder, and 100 parts of glass fiber to mix thoroughly for 20 minutes, add the mixed materials, add while stirring, mix for 5 minutes, and package after mixing.

[0043] Example 5

[0044] The method for preparing the molding material for the waterproof and breathable flower pot of this embodiment comprises the following steps:

[0045] A. Premix 100 parts of a base resin with a low styrene content with 200 parts of purple clay, and mix them using an open mill to form a state where no individual powder falls but no excess resin, i.e., a premix; place the mixed material in a vacuum drying oven at 55°C, with a vacuum degree of 0.2Mpa, and a vacuum drying time of 6 hours, and evacuate the system to form pores;

[0046] B. 100 parts of the base resin are mixed with 8 parts of the initiator TBPB, 3 parts of the rheology modifier carbon diamide MgO, and 5 parts of the release agent calcium stearate, and dispersed using a high-speed disperser with an adjustable speed of 1000 rpm for 15 minutes to prepare a resin paste for molding material;

[0047] C. Use resin paste, 3 parts of carbon black, and 250 parts of glass fiber to mix thoroughly for 20 minutes, add the mixed materials, add while stirring, mix for 5 minutes, and package after mixing.

[0048] Comparative Example 1

[0049] The molding compound preparation method of this comparative example comprises the following steps:

[0050] A. 200 parts of the base resin are mixed with 10 parts of the initiator TBPB, 1 part of the rheology modifier MgO, and 15 parts of the release agent calcium stearate, and dispersed using a high-speed disperser with an adjustable speed of 1000 rpm for 15 minutes to prepare a resin paste for molding material;

[0051] B. Use resin paste, 300 parts of filler calcium carbonate, and 100 parts of glass fiber to mix thoroughly for 20 minutes. After mixing, package and make sample C.

[0052] Comparative Example 2

[0053] The molding compound preparation method of this comparative example comprises the following steps:

[0054] A. 200 parts of the base resin are mixed with 10 parts of the initiator TBPB, 1 part of the rheology modifier MgO, and 15 parts of the release agent calcium stearate, and dispersed using a high-speed disperser with an adjustable speed of 1000 rpm for 15 minutes to prepare a resin paste for molding material;

[0055] B. Use resin paste, 100 parts of red clay, 300 parts of filler calcium carbonate, and 100 parts of glass fiber to mix thoroughly for 20 minutes, and package after mixing.

[0056] Table 1 Example group distribution ratio table

[0057]

[0058] The molding materials of Examples 1 to 5 of the present invention and Comparative Examples 1 and 2 were tested for tensile strength, water impermeability and water vapor permeability. The test method for tensile strength adopts the enterprise standard JF03-47-2012 "Technical Conditions for Supply of SMC Products for Automobiles" of China First Automobile Co., Ltd. to measure five samples and calculate the average value. When sampling and testing the mechanical strength of the molding material, due to the large discreteness of the mechanical strength, it is necessary to take multiple samples to calculate the average value. It is normal for the same set of data to fluctuate by about 10%. The water impermeability experiment uses a water column with a height of 1000mm for 2h to see if the water column level drops. The water vapor permeability is measured using GB / T1037-1988 "Test Method for Water Vapor Permeability of Plastic Film and Sheet---Cup Method" (corresponding to the American Testing and Association Standard ASTM E96-1980). Under the conditions of specified temperature, relative humidity, a certain water vapor pressure difference and a certain thickness, 1m 2 The amount of water vapor that passes through a sample within 24 hours.

[0059] Table 2 Test data table

[0060]

[0061] From the data in Table 2, it can be seen that the water vapor permeability of the molding material prepared by the present invention is greatly improved compared with the existing molding material with a water vapor permeability of 0, that is, the flower pot prepared by the molding material has strong waterproof and breathable properties, can effectively simulate the living environment of plants in the land, is more suitable for plant growth, and can reduce the requirements for plant survival soil.

[0062] The unsaturated polyester resin and vinyl resin used in the present invention are conventional unsaturated polyester resin and vinyl resin, which are produced by the enterprise itself.

[0063] Obviously, the above embodiments are merely examples for clearly explaining the present invention, and are not intended to limit the implementation methods of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. However, these obvious changes or modifications derived from the spirit of the present invention are still within the scope of protection of the present invention.

Claims

1. A molding compound for waterproof and breathable flower pots, It is characterized in that The invention comprises the following components in percentage by mass: 15-50% of a pretreated resin-clay mixture, 9-20% of a matrix resin, 20-75% of a filler, 0.5-1.5% of an initiator, 0.1-1% of a rheology regulator, 0.5-3% of an auxiliary agent and 0-30% of a reinforcing fiber; the sum of the percentages by mass of the pretreated resin-clay mixture, the matrix resin, the filler, the initiator, the rheology regulator, the auxiliary agent and the reinforcing fiber is 100%; the pretreated resin-clay mixture is prepared by mixing a high-solid content resin with clay and then vacuum drying the mixture to form a pretreated resin-clay mixture having a porous structure; the high-solid content resin has a resin solid content greater than 80%, the mass ratio of the high-solid content resin to the clay is 1:2-1:1, and the mass of the clay is not less than 10% of the total mass of the molding material; the high-solid content resin and the matrix resin are unsaturated polyester resin or vinyl resin.

2. The molding compound for waterproof and breathable flower pot according to claim 1, It is characterized in that The pottery clay is one or more of purple clay, red clay, white clay, and yellow clay.

3. The molding compound for waterproof and breathable flowerpot according to claim 1, It is characterized in that The filler is one or more of calcium carbonate, aluminum hydroxide and barium sulfate.

4. The molding material for waterproof and breathable flower pot according to claim 3, It is characterized in that The high-solid content resin and the base resin contain unsaturated cross-linking monomers; the unsaturated cross-linking monomers are one or more of styrene, vinyl toluene, α-methylstyrene, vinyl chloride benzene, divinyl benzene, diallyl phthalate and methyl methacrylate; the mass of the unsaturated cross-linking monomers in the high-solid content resin is not more than 20% of the total mass of the high-solid content resin, and the mass of the unsaturated cross-linking monomers in the base resin accounts for 30-50% of the total mass of the base resin; the filler contains one or more of graphite, carbon black, carbon nanotubes, graphene, elemental silicon powder, silicon dioxide powder, mica, fly ash and glass beads.

5. The molding compound for a waterproof and breathable flower pot according to any one of claims 1 to 4, It is characterized in that The initiator is one or more of tert-butyl perbenzoate, diacetyl peroxide, dibenzoyl peroxide, peroxyoctanoate and tert-butyl perbenzoate; The rheology modifier is one or more of alkaline earth metal oxides, alkaline earth metal hydroxides, carbodiamide, aziridine, polyisocyanate, polytetrafluoroethylene, perfluoropolyether, polyethylene, clay and fumed silica; The auxiliary agent is one or more of a release agent, a dispersant, a viscosity reducer, and a defoaming agent.

6. The molding compound for a waterproof and breathable flower pot according to any one of claims 1 to 4, It is characterized in that The reinforcing fiber is one or more of glass fiber, carbon fiber and aramid fiber.

7. A method for preparing the molding material for waterproof and breathable flower pots as claimed in claim 1, It is characterized in that The following steps are involved: A. Premix the high solid content resin and clay, and place the obtained premix in a vacuum drying oven at a temperature of 50°C to 60°C, with a vacuum degree of 0.2 to 0.6 MPa, and a vacuum drying time of 2 to 6 hours to form a pretreated resin-clay mixture with a porous structure; B. Mix the base resin, initiator, rheology modifier and additives, and disperse them using a high-speed disperser to obtain a resin paste; C. After mixing the resin paste, filler and reinforcing fiber, add the pretreated resin clay mixture and continue mixing to obtain a molding compound.

8. The method for preparing the molding compound for waterproof and breathable flower pots according to claim 7, It is characterized in that The rotation speed of the high-speed dispersion in step B is 1000-1500 rpm, and the dispersion time is at least 10 minutes.

9. The method for preparing the molding compound for waterproof and breathable flower pots according to claim 7, It is characterized in that In the step C, the resin paste, filler and reinforcing fiber are first mixed for 15 to 30 minutes, and then the pretreated resin clay mixture is added and mixed for 2 to 5 minutes.

Citation Information

Patent Citations

  • Ceramic flowerpot and manufacturing technology thereof

    CN107555946A

  • Method for improving saline-alkali soil and planting method in saline-alkali soil

    CN108496454A