Solvent-free polyurethane leather for car mats, preparation method thereof, and car mats

Through the combination of solvent-free polyurethane leather and radiation-proof filler, the material performance and environmental protection issues of automobile floor mats are solved, the preparation of zero-emission, wear-resistant, and radiation-resistant automobile floor mats is achieved, and the mechanical properties and user safety of the product are improved.

CN115928452BActive Publication Date: 2024-10-01SHANXI XINHONGBAO AUTOMOBILE PROD CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211476482.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-23
Publication Date
2024-10-01
Estimated Expiration
2042-11-23

AI Technical Summary

Technical Problem

Existing automobile floor mat materials have problems such as environmental protection, no odor, insufficient wear resistance and comfort performance, and the traditional preparation process produces waste gas and waste water, which increases production costs and environmental pollution.

Method used

Solvent-free polyurethane leather is used as the surface material, which is directly coated on the base fabric through a polyester-polyether copolymer system, and radiation-proof fillers are added. No waste gas or waste water is produced during the preparation process, forming a zero-emission car mat with Solid, scratch-resistant, wear-resistant and stretchable product.

Benefits of technology

The car mats are realized to be solid in texture, scratch-resistant and wear-resistant, odor-free, delicate and soft to the touch, can effectively absorb and shield microwave and electromagnetic wave radiation, improve mechanical properties, and meet environmental protection and performance requirements.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a solvent-free polyurethane leather for automobile foot pads, a preparation method thereof and an automobile foot pad, wherein the solvent-free polyurethane leather comprises a base fabric layer and a polyurethane surface layer, wherein the polyurethane surface layer comprises the following raw materials by weight: 50-80 parts of polyester polyols, 20-30 parts of polyether polyols, 5-10 parts of chain extenders, 0.1-2 parts of catalysts, 50-80 parts of diisocyanates, 5-15 parts of triisocyanates, 1-3 parts of foaming agents, 0.5-1 parts of foam stabilizers, 0.5-1.5 parts of leveling agents, and 10-20 parts of radiation-proof fillers. The polyurethane leather raw materials are free of solvents, plasticizers, and heavy metals, and waste gas and waste water are not generated during the production process, so that zero emission is achieved. The prepared foot pad has a solid texture, is scratch-resistant and wear-resistant, has good stretchability, is not easily deformed, has no odor, and has a delicate and soft feel. It can effectively absorb, shield, and attenuate a large amount of microwave and electromagnetic wave radiation of the vehicle body itself, and prevents the possible harm of radiation to the human body, and also has good mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of automobile foot pad preparation, and particularly relates to a solvent-free polyurethane leather for automobile foot pads, a preparation method thereof, and the automobile foot pad. Background Art

[0002] Car floor mats are an environmentally friendly automotive interior component that integrates five main functions: water absorption, dust absorption, dirt removal, sound insulation, and protection of the main body carpet. Car floor mats are interior decorations that protect the cleanliness of the inside and outside of the car and play a role in aesthetic and comfortable embellishment. Car floor mats absorb water, dust, and dirt, which can effectively prevent the residual moisture and dirt on the soles from sliding with the clutch, brake, and accelerator, avoid safety hazards, and reduce the possibility of interior pollution and damage. After all, cleaning floor mats is more convenient and economical than cleaning interiors.

[0003] At present, there is no unified national standard or industry standard for car mats. There are many types of mats. Most of the materials used in high-end car mats are made of special rubber or silicone rubber. The multi-layer composite material with expanded paper as the middle layer has increased the production cost of the car mats and is not conducive to environmental protection. The production process of car mats sold on the market is generally complicated and the material cost is high. At the same time, people's performance requirements for car mats are getting higher and higher. The preparation process of traditional car mats is inseparable from the gluing process. This is not only not conducive to environmental protection, but also increases the processing cost of car mats, which indirectly affects the performance of car mats.

[0004] With the continuous improvement of living standards, people have put forward higher and higher requirements for the interior conditions of passenger cars, especially the functionality, aesthetics, comfort and green environmental protection performance of car interiors. At present, the automotive interior leather on the market is mainly composed of natural leather and PVC artificial leather. Natural leather is harmful to animals because it is made from animal skins, and is gradually resisted by animal protection organizations; while PVC artificial leather has shortcomings such as poor comfort, strong odor, and easy migration of plasticizers. In recent years, it has gradually been replaced by highly weather-resistant polyurethane (PU) synthetic leather. Solvent-based polyurethane synthetic leather products have the characteristics of breathability, waterproofness, softness, wear resistance, high strength, excellent hydrolysis resistance, etc., and their appearance and performance are close to natural leather. Its processing mainly consists of two parts: wet process and dry process. Determined by the characteristics of finished leather processing technology, the organic solvent N,N-dimethylformamide (DMF) used in the wet leather processing and dry bonding process is difficult to completely remove, resulting in a certain amount of DMF residue in the leather; with the increasing environmental pressure faced by solvent-based polyurethane synthetic leather, the development of greener polyurethane synthetic leather is imminent.

[0005] Chinese patent application No. 201710483380.2 discloses a car mat, which includes environmentally friendly recycled colored polyester fiber and low-melting polyester fiber. The present invention solves the technical problem of avoiding gluing of car interior materials, which not only makes the performance superior to traditional gluing car mats, but also makes the product more competitive. At the same time, it reduces the production process and reduces labor costs and material costs, so that the quality of the car mats is guaranteed, and it can also meet the large-scale production of car mats, and has good application prospects. However, the patent does not improve the raw materials of the mats, and it is impossible to know whether the prepared mats have environmental protection, no odor, good wear resistance and comfort. Therefore, in view of some problems existing in my country's car mats, this application invents a car mat to solve the above problems, which has good application prospects. Summary of the invention

[0006] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a solvent-free polyurethane leather for car mats, a preparation method thereof and a car mat. The car mat uses solvent-free leather as a surface material. The polyurethane leather raw material contains no solvent, no plasticizer and no heavy metal. No waste gas or waste water is generated during the production process, thus achieving zero emission. The prepared mat has a solid texture, is scratch-resistant and wear-resistant, has good stretchability, is not easy to deform, has no odor, and has a delicate and soft touch. It can effectively absorb, shield and attenuate a large amount of microwave and electromagnetic wave radiation from the car body itself, thereby preventing possible harm to the human body caused by the radiation, and also has good mechanical properties.

[0007] To achieve the above object, the present invention provides the following technical solutions:

[0008] A solvent-free polyurethane leather for automobile foot pads comprises a base fabric layer and a polyurethane surface layer. The polyurethane surface layer comprises the following raw materials in parts by weight: 50-80 parts of polyester polyol, 20-30 parts of polyether polyol, 5-10 parts of chain extender, 0.1-2 parts of catalyst, 50-80 parts of diisocyanate, 5-15 parts of triisocyanate, 1-3 parts of foaming agent, 0.5-1 parts of foam stabilizer, 0.5-1 parts of leveling agent and 10-20 parts of radiation protection filler.

[0009] Preferably, the polyester polyol is one or more of polyneopentyl adipate diol, poly1,4-butylene adipate diol, and polymethyl propane adipate diol; the polyether polyol is one or more of polyoxypropylene diol, polytetrahydrofuran diol, and tetrahydrofuran-oxypropylene copolymer diol; the chain extender is one or more of ethylene glycol, 1,3-propylene glycol, and 1,4-butylene glycol; the catalyst is one or more of stannous octoate, dibutyltin dilaurate, zinc isooctanoate, and bismuth isooctanoate.

[0010] Preferably, the diisocyanate is one or more of 2,4-toluene diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate, and 4,4'-diphenylmethane diisocyanate; the triisocyanate is HDI trimer; the foaming agent is water or cyclopentane; the foam stabilizer is polyether silicone oil; and the leveling agent is one or more of BYK-322, BYK-333, and BYK-345.

[0011] Preferably, the method for preparing the radiation-proof filler comprises the following steps:

[0012] (1) adding illite and diatomite to hydrochloric acid for impregnation, washing and drying after the impregnation to obtain a mixed powder, then mixing the mixed powder with ferric chloride, calcining in a muffle furnace, washing, drying, grinding, and sieving after the calcination to obtain an iron-activated mixed powder;

[0013] (2) adding the iron activated mixed powder obtained in step (1) into a barium chloride solution, immersing at 30-50° C. for 12 h, then dropping a sodium sulfate solution under stirring, filtering, washing, and drying after the dropping is completed to obtain modified particles;

[0014] (3) uniformly mixing the modified particles, lanthanum oxide and polycarbosilane in step (2), and performing melt spinning to obtain continuous polycarbosilane fibers, and then electron irradiating the polycarbosilane fibers under nitrogen protection, and then performing high-temperature sintering and low-temperature pulverizing under nitrogen protection to obtain inorganic particles / cross-linked silicon carbide fiber powder;

[0015] (4) Add the inorganic particles / cross-linked silicon carbide fiber powder obtained in step (3) into anhydrous ethanol, then add phthalic anhydride, soak at room temperature for 2-4 hours, then add zirconate coupling agent, stir to react, filter and dry after the reaction is completed to obtain a radiation-proof filler.

[0016] Preferably, in step (1), the mass ratio of illite, diatomite and ferric chloride is 20:10-30:5-10; the mass concentration of hydrochloric acid is 10-15%; the calcination temperature is 700-800°C, and the calcination time is 3-5h; the concentration of the barium chloride solution in step (2) is 0.1-0.5mol / L, and the concentration of the sodium sulfate solution is 0.1-0.5mol / L; the mass volume ratio of the mixed powder, barium chloride solution and sodium sulfate solution is 30g:200-400mL:200-400mL; and the stirring speed is 300-500r / min.

[0017] Preferably, in step (3), the mass ratio of the modified particles, lanthanum oxide and polycarbosilane is 10-15:4-8:100; the temperature of the melt spinning is 280-320°C; the electron irradiation dose is 8-12MGy; the temperature of the high-temperature sintering is 1300-1500°C, and the sintering time is 3-6h; the temperature of the low-temperature crushing is below -50°C.

[0018] Preferably, in step (4), the mass ratio of the inorganic particles / cross-linked silicon carbide fibers, phthalic anhydride, and zirconate coupling agent is 100:10-15:3-6; the stirring reaction temperature is 50-70°C, and the reaction time is 3-5h.

[0019] The present invention also protects a method for preparing the solvent-free polyurethane leather for automobile mats, comprising the following steps:

[0020] (a) weighing raw materials according to the formula, adding polyester polyol, polyether polyol, chain extender, foaming agent, foam stabilizer, leveling agent and catalyst into a reaction kettle, stirring and reacting to obtain component A;

[0021] (b) adding diisocyanate, triisocyanate and radiation protection filler to component A of step (a), heating and reacting, cooling after the reaction is completed to obtain a slurry, and then coating the slurry on the surface of the release paper at a coating amount of 150-200 g / m2, and drying to form a polyurethane surface layer;

[0022] (c) laminating the base fabric layer and the polyurethane surface layer in step (b) and pressing them together with a laminating roller. After lamination, the laminating process is completed and the laminating process is carried out in an oven for aging. After aging, the release paper is peeled off and the solvent-free polyurethane leather is obtained.

[0023] Preferably, the stirring reaction temperature in step (a) is 60-90°C, the reaction time is 3-5h, and the stirring speed is 60-100r / min; the heating reaction temperature in step (b) is 70-90°C, the reaction time is 0.5-1h, and the drying conditions are 3-5min at 100-120°C; the laminating roller pressure in step (c) is 1-3MPa, and the oven aging conditions are 130-150°C oven aging for 8-12min.

[0024] The present invention also protects a car mat, which comprises, from top to bottom, the solvent-free polyurethane leather layer, the high-density high-elastic foam layer, the non-woven fabric layer, the TPU hot-melt film layer, the TPU high-temperature resistant film layer, the adhesive resin layer, the high-gloss PET release film layer, and the environmentally friendly PP synthetic paper layer;

[0025] Wherein, the high-density and high-elastic foam layer is electron irradiated cross-linked polyethylene foam with a density of 0.1-0.2 kg / cm3 and a thickness of 0.5-1 mm; the thickness of the non-woven fabric layer is 0.1-0.2 mm.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] (1) The solvent-free polyurethane leather for automobile floor mats provided by the present invention is directly coated on the base fabric with a solvent-free polyurethane of a polyester-polyether copolymer system, which can effectively ensure the high-temperature durability and various mechanical properties of the polyurethane leather while meeting the hydrolysis resistance of the polyurethane leather product. In the post-curing cross-linking process, triisocyanate can cross-link the linear polyurethane to form a bulk polymer with a higher molecular weight, thereby ensuring the wear resistance, scratch resistance, water resistance, solvent resistance and other thermodynamic mechanical properties of the polyurethane leather.

[0028] (2) The solvent-free polyurethane leather for automobile floor mats provided by the present invention improves the absorption of polyurethane leather and shields a large amount of microwave and electromagnetic wave radiation of the car body itself by adding radiation-proof fillers; first, illite and diatomaceous earth are mixed and added to hydrochloric acid for immersion to weaken the interlayer bonding force of illite, so as to facilitate the intercalation of organic molecules or the attachment of organic molecules to the surface of illite. At the same time, after the acid treatment, the surface defects of illite increase, providing more reaction sites for subsequent modification, thereby improving the modification effect, and the acid treatment also removes impurities in diatomaceous earth, exposing its microporous structure, expanding its pore size, and facilitating the coating of barium sulfate; then, ferric chloride and the mixed powder are calcined to replace the iron ions with Al in the illite crystal layer, thereby improving the electronegativity of the illite. The negative charge of the layer surface can limit the movement of cations to a certain extent, so that it has stronger molecular adsorption capacity in the subsequent steps; then, the iron-activated mixed powder is calcined in chloride The mixed powder is immersed in a barium sulfate solution, sodium sulfate is added, and barium sulfate is coated on the surface of the mixed powder. The barium element core in barium sulfate has a large mass, a large number of atoms per unit volume, a high probability of photoelectric effect, and easy absorption of radiation energy. At the same time, barium ions have a high dielectric constant or magnetization intensity, and have a strong magnetic loss effect on electromagnetic radiation, so that the mixed powder has a higher radiation shielding performance; then the modified particles, lanthanum oxide and polycarbosilane are spun, cross-linked under irradiation conditions, and sintered to obtain inorganic particles / cross-linked silicon carbide fibers. The cross-linked silicon carbide fibers are all structural absorbing materials, which can not only absorb electromagnetic waves and reduce echo energy, but also can be made into structural parts that withstand compression, bending and shear loads. Finally, the cross-linked silicon carbide fibers and inorganic particles are modified with coupling agents to have better dispersibility and adhesion in solvent-free polyurethane, and are not easy to fall off, thereby improving the mechanical properties of polyurethane leather.

[0029] (3) The automobile floor mat provided by the present invention uses solvent-free polyurethane leather as the surface material. The polyurethane leather raw material contains no solvent, no plasticizer, and no heavy metal. No waste gas or waste water is generated during the production process, thus achieving zero emission. The prepared floor mat has a solid texture, is scratch-resistant and wear-resistant, has good stretchability, is not easy to deform, has no odor, and has a delicate and soft feel. It can effectively absorb, shield, and attenuate a large amount of microwave and electromagnetic wave radiation from the vehicle body itself, thereby preventing possible harm to the human body caused by radiation. At the same time, it also has good mechanical properties. DETAILED DESCRIPTION

[0030] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] The polyether silicone oil was purchased from Guangzhou Yinuo Chemical Technology Co., Ltd. with the brand name Dow Corning SF-8427; the polycarbosilane was purchased from Suzhou Sailifeitao Fiber Co., Ltd. with a number average molecular weight of 1300-1500 and a softening point of 207-219°C; the illite was purchased from Lingshou Antai Mining Co., Ltd. with a mesh size of 325 mesh; the diatomaceous earth was purchased from Hebei Jiegui Mineral Products Co., Ltd. with a mesh size of 325 mesh; the lanthanum oxide was purchased from Jiangsu Runfeng Synthetic Technology Co., Ltd. with a material diameter of 20-30 μm; the barium sulfate was purchased from Shandong Xinfayuan Metal Materials Co., Ltd. with a particle size of 1-10 μm; the silicon carbide powder was purchased from Gongyi Yuying Refractory Materials Co., Ltd. with a mesh size of 325 mesh.

[0032] Example 1

[0033] A method for preparing solvent-free polyurethane leather for automobile foot pads comprises the following steps:

[0034] (a) weighing raw materials according to the formula, adding 70 parts of polyneopentyl adipate diol, 25 parts of polytetrahydrofuran diol, 8 parts of 1,3-propylene glycol, 2 parts of water, 0.8 parts of polyether silicone oil, 1 part of BYK-333 and 1 part of stannous octoate into a reaction kettle, stirring and reacting at 80° C. and 80 r / min for 4 hours to obtain component A;

[0035] (b) adding 70 parts of isophorone diisocyanate, 10 parts of HDI trimer and 15 parts of radiation protection filler to component A of step (a), reacting at 80° C. for 1 hour, cooling after the reaction is completed to obtain a slurry, and then coating the slurry on the surface of the release paper with a coating amount of 180 g / m2, and baking at 110° C. for 4 minutes to form a polyurethane surface layer;

[0036] (c) The base fabric layer is laminated with the polyurethane surface layer in step (b) and then pressed with a laminating roller. The laminating roller pressure is 2 MPa. After the lamination is completed, the leather is put into an oven for aging. The oven aging condition is 140° C. for 10 min. After aging, the leather is cooled and the release paper is peeled off to obtain the solvent-free polyurethane leather.

[0037] The method for preparing the radiation-proof filler comprises the following steps:

[0038] (1) 20 g of illite and 20 g of diatomite were added to 500 mL of 15% hydrochloric acid and immersed for 5 h. After the immersion, the mixture was washed and dried to obtain a mixed powder. Subsequently, the mixed powder was mixed evenly with 8 g of ferric chloride and calcined in a muffle furnace at a calcination temperature of 750° C. for 4 h. After the calcination, the mixture was washed, dried, ground and sieved to obtain an iron-activated mixed powder.

[0039] (2) adding the iron activated mixed powder (30 g) obtained in step (1) into 300 mL of 0.3 mol / L barium chloride solution, immersing at 40° C. for 12 h, then dropping 300 mL of 0.3 mol / L sodium sulfate solution at a stirring speed of 400 r / min, filtering, washing and drying after the dropping to obtain modified particles;

[0040] (3) The modified particles (13 g), 6 g of lanthanum oxide and 100 g of polycarbosilane in step (2) are mixed uniformly, and melt-spinned to obtain continuous polycarbosilane fibers at a temperature of 300° C. The polycarbosilane fibers are then electron irradiated under nitrogen protection at a dose of 10 MGy, and then high-temperature sintered and low-temperature crushed under nitrogen protection at a temperature of 1400° C. for 5 h and a low-temperature crushing temperature of -70° C. to obtain inorganic particles / cross-linked silicon carbide fiber powder;

[0041] (4) The inorganic particles / cross-linked silicon carbide fiber powder (100 g) obtained in step (3) was added to 700 mL of anhydrous ethanol, followed by the addition of 13 g of phthalic anhydride, and the mixture was immersed at room temperature for 3 h. Then, 5 g of zirconate coupling agent was added, and the mixture was stirred at 60 ° C for 4 h. After the reaction was completed, the mixture was filtered and dried to obtain a radiation-proof filler.

[0042] Example 2

[0043] A method for preparing solvent-free polyurethane leather for automobile foot pads comprises the following steps:

[0044] (a) weighing the raw materials according to the formula, adding 50 parts of poly(1,4-butylene adipate diol), 20 parts of polyoxypropylene glycol, 5 parts of ethylene glycol, 1 part of cyclopentane, 0.5 parts of polyether silicone oil, 0.5 parts of BYK-322 and 0.1 parts of dibutyltin dilaurate into a reaction kettle, stirring and reacting at 60° C. and 60 r / min for 5 hours to obtain component A;

[0045] (b) adding 50 parts of 2,4-toluene diisocyanate, 5 parts of HDI trimer, and 10 parts of radiation protection filler to component A of step (a), reacting at 70° C. for 1 hour, cooling after the reaction is completed to obtain a slurry, and then coating the slurry on the surface of the release paper with a coating amount of 150 g / m2, and baking at 100° C. for 5 minutes to form a polyurethane surface layer;

[0046] (c) The base fabric layer is laminated with the polyurethane surface layer in step (b) and then pressed with a laminating roller. The laminating roller pressure is 1 MPa. After the lamination is completed, the leather is put into an oven for aging at 130° C. for 12 min. After aging, the leather is cooled and the release paper is peeled off to obtain the solvent-free polyurethane leather.

[0047] The method for preparing the radiation-proof filler comprises the following steps:

[0048] (1) 20 g of illite and 10 g of diatomite were added to 500 mL of 10% hydrochloric acid and immersed for 6 h. After the immersion, the mixture was washed and dried to obtain a mixed powder. Subsequently, the mixed powder was mixed evenly with 5 g of ferric chloride and calcined in a muffle furnace at a calcination temperature of 700 ° C. for 5 h. After the calcination, the mixture was washed, dried, ground and sieved to obtain an iron-activated mixed powder.

[0049] (2) adding the iron activated mixed powder (30 g) obtained in step (1) into 200 mL of 0.5 mol / L barium chloride solution, immersing at 30° C. for 12 h, then dropping 200 mL of 0.5 mol / L sodium sulfate solution at a stirring speed of 300 r / min, filtering, washing and drying after the dropping to obtain modified particles;

[0050] (3) The modified particles (10 g), 4 g lanthanum oxide and 100 g polycarbosilane in step (2) are mixed uniformly, and melt-spinned to obtain continuous polycarbosilane fibers at a melt-spinning temperature of 280° C. The polycarbosilane fibers are then electron-irradiated under nitrogen protection at an irradiation dose of 8 MGy, and then high-temperature sintered and low-temperature crushed under nitrogen protection at a temperature of 1300° C. for 6 h and a low-temperature crushing temperature of -50° C. to obtain inorganic particles / cross-linked silicon carbide fiber powder;

[0051] (4) The inorganic particles / cross-linked silicon carbide fiber powder (100 g) obtained in step (3) was added to 700 mL of anhydrous ethanol, followed by 10 g of phthalic anhydride, and immersed at room temperature for 2 h. Then, 3 g of zirconate coupling agent was added, and the mixture was stirred at 50 ° C for 5 h. After the reaction was completed, the mixture was filtered and dried to obtain a radiation-proof filler.

[0052] Example 3

[0053] A method for preparing solvent-free polyurethane leather for automobile foot pads comprises the following steps:

[0054] (a) weighing the raw materials according to the formula, adding 80 parts of poly(methyl propylene adipate) glycol, 30 parts of tetrahydrofuran-propylene oxide copolymer glycol, 10 parts of 1,4-butanediol, 3 parts of water, 1 part of polyether silicone oil, 1.5 parts of BYK-345 and 2 parts of bismuth isooctanoate into a reaction kettle, stirring and reacting at 90° C. and 100 r / min for 3 hours to obtain component A;

[0055] (b) adding 80 parts of 4,4'-diphenylmethane diisocyanate, 15 parts of HDI trimer, and 20 parts of radiation protection filler to component A of step (a), reacting at 90°C for 0.5h, cooling after the reaction to obtain a slurry, and then coating the slurry on the surface of the release paper with a coating amount of 200g / m2, and baking at 120°C for 3min to form a polyurethane surface layer;

[0056] (c) The base fabric layer is laminated with the polyurethane surface layer in step (b) and then pressed with a laminating roller. The laminating roller pressure is 3 MPa. After the lamination is completed, the leather is put into an oven for aging at 150° C. for 8 min. After aging, the leather is cooled and the release paper is peeled off to obtain the solvent-free polyurethane leather.

[0057] The method for preparing the radiation-proof filler comprises the following steps:

[0058] (1) 20 g of illite and 30 g of diatomite were added to 500 mL of 15% hydrochloric acid and immersed for 3 h. After the immersion, the mixture was washed and dried to obtain a mixed powder. Subsequently, the mixed powder was evenly mixed with 10 g of ferric chloride and calcined in a muffle furnace at a calcination temperature of 800 ° C. for 3 h. After the calcination, the mixture was washed, dried, ground and sieved to obtain an iron-activated mixed powder.

[0059] (2) adding the iron activated mixed powder (30 g) obtained in step (1) into 400 mL of 0.1 mol / L barium chloride solution, immersing at 50° C. for 12 h, then dropping 400 mL of 0.1 mol / L sodium sulfate solution at a stirring speed of 500 r / min, filtering, washing and drying after the dropping to obtain modified particles;

[0060] (3) The modified particles (15 g), 8 g of lanthanum oxide and 100 g of polycarbosilane in step (2) are mixed uniformly, and melt-spinned to obtain continuous polycarbosilane fibers at a melt spinning temperature of 320° C. The polycarbosilane fibers are then electron irradiated under nitrogen protection at an irradiation dose of 12 MGy, and then high-temperature sintered and low-temperature crushed under nitrogen protection at a temperature of 1500° C. for 3 h and a low-temperature crushing temperature of -80° C. to obtain inorganic particles / cross-linked silicon carbide fiber powder;

[0061] (4) The inorganic particles / cross-linked silicon carbide fiber powder (100 g) obtained in step (3) was added to 700 mL of anhydrous ethanol, followed by 15 g of phthalic anhydride, and immersed at room temperature for 4 h. Then, 6 g of zirconate coupling agent was added, and the mixture was stirred at 70 ° C for 3 h. After the reaction was completed, the mixture was filtered and dried to obtain a radiation-proof filler.

[0062] Comparative Example 1

[0063] A method for preparing solvent-free polyurethane leather for automobile foot pads comprises the following steps:

[0064] (a) weighing raw materials according to the formula, adding 70 parts of polyneopentyl adipate diol, 25 parts of polytetrahydrofuran diol, 8 parts of 1,3-propylene glycol, 2 parts of water, 0.8 parts of polyether silicone oil, 1 part of BYK-333 and 1 part of stannous octoate into a reaction kettle, stirring and reacting at 80° C. and 80 r / min for 4 hours to obtain component A;

[0065] (b) adding 70 parts of isophorone diisocyanate, 10 parts of HDI trimer and 15 parts of radiation protection filler to component A of step (a), reacting at 80° C. for 1 hour, cooling after the reaction is completed to obtain a slurry, and then coating the slurry on the surface of the release paper with a coating amount of 180 g / m2, and baking at 110° C. for 4 minutes to form a polyurethane surface layer;

[0066] (c) The base fabric layer is laminated with the polyurethane surface layer in step (b) and then pressed with a laminating roller. The laminating roller pressure is 2 MPa. After the lamination is completed, the leather is put into an oven for aging. The oven aging condition is 140° C. for 10 min. After aging, the leather is cooled and the release paper is peeled off to obtain the solvent-free polyurethane leather.

[0067] The method for preparing the radiation-proof filler comprises the following steps:

[0068] (1) 20 g of illite and 20 g of diatomite were added to 500 mL of 15% hydrochloric acid and immersed for 5 h. After the immersion, the mixture was washed and dried to obtain a mixed powder.

[0069] (2) The mixed powder (13 g) in step (1), 5 g of barium sulfate, 6 g of lanthanum oxide, and 100 g of polycarbosilane are uniformly mixed, and melt-spinned to obtain continuous polycarbosilane fibers at a melt spinning temperature of 300° C. The polycarbosilane fibers are then electron irradiated under nitrogen protection at an irradiation dose of 10 MGy, and then high-temperature sintered and low-temperature crushed under nitrogen protection at a temperature of 1400° C. for 5 h and a low-temperature crushing temperature of -70° C. to obtain inorganic particles / cross-linked silicon carbide fiber powder;

[0070] (3) The inorganic particles / cross-linked silicon carbide fiber powder (100 g) obtained in step (2) was added to 700 mL of anhydrous ethanol, followed by the addition of 13 g of phthalic anhydride, and the mixture was immersed at room temperature for 3 h. Then, 5 g of zirconate coupling agent was added, and the mixture was stirred at 60 ° C for 4 h. After the reaction was completed, the mixture was filtered and dried to obtain a radiation-proof filler.

[0071] Comparative Example 2

[0072] A method for preparing solvent-free polyurethane leather for automobile foot pads comprises the following steps:

[0073] (a) weighing raw materials according to the formula, adding 70 parts of polyneopentyl adipate diol, 25 parts of polytetrahydrofuran diol, 8 parts of 1,3-propylene glycol, 2 parts of water, 0.8 parts of polyether silicone oil, 1 part of BYK-333 and 1 part of stannous octoate into a reaction kettle, stirring and reacting at 80° C. and 80 r / min for 4 hours to obtain component A;

[0074] (b) adding 70 parts of isophorone diisocyanate, 10 parts of HDI trimer and 15 parts of radiation protection filler to component A of step (a), reacting at 80° C. for 1 hour, cooling after the reaction is completed to obtain a slurry, and then coating the slurry on the surface of the release paper with a coating amount of 180 g / m2, and baking at 110° C. for 4 minutes to form a polyurethane surface layer;

[0075] (c) The base fabric layer is laminated with the polyurethane surface layer in step (b) and then pressed with a laminating roller. The laminating roller pressure is 2 MPa. After the lamination is completed, the leather is put into an oven for aging. The oven aging condition is 140° C. for 10 min. After aging, the leather is cooled and the release paper is peeled off to obtain the solvent-free polyurethane leather.

[0076] The method for preparing the radiation-proof filler comprises the following steps:

[0077] (1) 20 g of illite and 20 g of diatomite were added to 500 mL of 15% hydrochloric acid and immersed for 5 h. After the immersion, the mixture was washed and dried to obtain a mixed powder. Subsequently, the mixed powder was mixed evenly with 8 g of ferric chloride and calcined in a muffle furnace at a calcination temperature of 750° C. for 4 h. After the calcination, the mixture was washed, dried, ground and sieved to obtain an iron-activated mixed powder.

[0078] (2) adding the iron activated mixed powder (30 g) obtained in step (1) into 300 mL of 0.3 mol / L barium chloride solution, immersing at 40° C. for 12 h, then dropping 300 mL of 0.3 mol / L sodium sulfate solution at a stirring speed of 400 r / min, filtering, washing and drying after the dropping to obtain modified particles;

[0079] (3) mixing the modified particles (13 g) in step (2), 6 g of lanthanum oxide, and 10 g of silicon carbide powder to obtain composite inorganic particles;

[0080] (4) The inorganic particles / cross-linked silicon carbide fiber powder (100 g) obtained in step (3) was added to 700 mL of anhydrous ethanol, followed by the addition of 13 g of phthalic anhydride, and the mixture was immersed at room temperature for 3 h. Then, 5 g of zirconate coupling agent was added, and the mixture was stirred at 60 ° C for 4 h. After the reaction was completed, the mixture was filtered and dried to obtain a radiation-proof filler.

[0081] Comparative Example 3

[0082] A method for preparing solvent-free polyurethane leather for automobile foot pads comprises the following steps:

[0083] (a) weighing raw materials according to the formula, adding 70 parts of polyneopentyl adipate diol, 25 parts of polytetrahydrofuran diol, 8 parts of 1,3-propylene glycol, 2 parts of water, 0.8 parts of polyether silicone oil, 1 part of BYK-333 and 1 part of stannous octoate into a reaction kettle, stirring and reacting at 80° C. and 80 r / min for 4 hours to obtain component A;

[0084] (b) adding 70 parts of isophorone diisocyanate, 10 parts of HDI trimer and 15 parts of radiation protection filler to component A of step (a), reacting at 80° C. for 1 hour, cooling after the reaction is completed to obtain a slurry, and then coating the slurry on the surface of the release paper with a coating amount of 180 g / m2, and baking at 110° C. for 4 minutes to form a polyurethane surface layer;

[0085] (c) The base fabric layer is laminated with the polyurethane surface layer in step (b) and then pressed with a laminating roller. The laminating roller pressure is 2 MPa. After the lamination is completed, the leather is put into an oven for aging. The oven aging condition is 140° C. for 10 min. After aging, the leather is cooled and the release paper is peeled off to obtain the solvent-free polyurethane leather.

[0086] The method for preparing the radiation-proof filler comprises the following steps:

[0087] (1) 20 g of illite and 20 g of diatomite were added to 500 mL of 15% hydrochloric acid and immersed for 5 h. After the immersion, the mixture was washed and dried to obtain a mixed powder. Subsequently, the mixed powder was mixed evenly with 8 g of ferric chloride and calcined in a muffle furnace at a calcination temperature of 750° C. for 4 h. After the calcination, the mixture was washed, dried, ground and sieved to obtain an iron-activated mixed powder.

[0088] (2) adding the iron activated mixed powder (30 g) obtained in step (1) into 300 mL of 0.3 mol / L barium chloride solution, immersing at 40° C. for 12 h, then dropping 300 mL of 0.3 mol / L sodium sulfate solution at a stirring speed of 400 r / min, filtering, washing and drying after the dropping to obtain modified particles;

[0089] (3) The modified particles (13 g), 6 g of lanthanum oxide and 100 g of polycarbosilane in step (2) are mixed evenly, and melt-spinned to obtain continuous polycarbosilane fibers at a temperature of 300°C. The polycarbosilane fibers are then electron irradiated under nitrogen protection at a dose of 10 MGy, and then high-temperature sintered and low-temperature crushed under nitrogen protection. The high-temperature sintering temperature is 1400°C, the sintering time is 5 hours, and the low-temperature crushing temperature is -70°C to obtain a radiation-proof filler.

[0090] The performance of the solvent-free polyurethane leather prepared in Examples 1-3 and Comparative Examples 1-3 was tested, and the internationally commonly used bow method was used to measure the reflectivity dB using an Agilent vector network analyzer. The test frequency range was 2-18 GHZ, and each sample was measured twice on the front side to obtain the average value. When the reflectivity dB is a negative value, the smaller the dB value, the better the wave absorption performance; the larger the dB value, the worse the wave absorption performance. The tensile strength was tested according to the GB / T 6344-2008 standard, the tear strength was tested according to the GB / T10808-2006 standard, and the peel strength was tested according to the GB / T 8949-2009 standard. The test results are shown in Table 1 below:

[0091] Table 1

[0092] Maximum reflection attenuation / -dB Tensile strength / MPa Tear strength / N Peel strength / N / 3cm Example 1 26.8 10.8 175 94 Example 2 24.5 9.3 173 86 Example 3 25.6 9.7 182 91 Comparative Example 1 15.2 7.8 160 81 Comparative Example 2 16.7 7.4 154 78 Comparative Example 3 21.3 5.7 137 63

[0093] As can be seen from Table 1 above, the solvent-free polyurethane leather prepared by the present invention has good microwave shielding and absorption properties, and also has good mechanical properties. However, in Comparative Example 1, since illite and diatomite are not replaced with iron ions and coated with barium sulfate, silicon carbide is not cross-linked in Comparative Example 2, and inorganic particles are not modified with coupling agents in Comparative Example 3, the various properties thereof are reduced, and the effects of the embodiments of the present invention cannot be achieved.

[0094] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A solvent-free polyurethane leather for automobile floor mats, comprising a base fabric layer and a polyurethane surface layer, characterized in that: The polyurethane surface layer comprises the following raw materials by weight: 50-80 parts of polyester polyol, 20-30 parts of polyether polyol, 5-10 parts of chain extender, 0.1-2 parts of catalyst, 50-80 parts of diisocyanate, 5-15 parts of triisocyanate, 1-3 parts of foaming agent, 0.5-1 parts of foam stabilizer, 0.5-1 parts of leveling agent, and 10-20 parts of radiation-proof filler; The preparation method of the radiation-proof filler comprises the following steps: (1) adding illite and diatomite to hydrochloric acid for impregnation, washing and drying after the impregnation to obtain a mixed powder, then mixing the mixed powder with ferric chloride, calcining in a muffle furnace, washing, drying, grinding, and sieving after the calcination to obtain an iron-activated mixed powder; (2) adding the iron activated mixed powder obtained in step (1) into a barium chloride solution, immersing at 30-50° C. for 12 h, then dropping a sodium sulfate solution under stirring, filtering, washing, and drying after the dropping is completed to obtain modified particles; (3) uniformly mixing the modified particles, lanthanum oxide and polycarbosilane in step (2), and performing melt spinning to obtain continuous polycarbosilane fibers, and then electron irradiating the polycarbosilane fibers under nitrogen protection, and then performing high-temperature sintering and low-temperature pulverizing under nitrogen protection to obtain inorganic particles / cross-linked silicon carbide fiber powder; (4) Add the inorganic particles / cross-linked silicon carbide fiber powder obtained in step (3) into anhydrous ethanol, then add phthalic anhydride, soak at room temperature for 2-4 hours, then add zirconate coupling agent, stir to react, filter and dry after the reaction is completed to obtain a radiation-proof filler.

2. The solvent-free polyurethane leather for automobile mats according to claim 1, characterized in that: The polyester polyol is one or more of polyneopentyl adipate diol, poly1,4-butylene adipate diol, and polymethylpropylene adipate diol; the polyether polyol is one or more of polyoxypropylene diol, polytetrahydrofuran diol, and tetrahydrofuran-oxypropylene copolymer diol; the chain extender is one or more of ethylene glycol, 1,3-propylene glycol, and 1,4-butylene glycol; the catalyst is one or more of stannous octoate, dibutyltin dilaurate, zinc isooctanoate, and bismuth isooctanoate.

3. The solvent-free polyurethane leather for automobile mats according to claim 1, characterized in that: The diisocyanate is one or more of 2,4-toluene diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate, and 4,4'-diphenylmethane diisocyanate; the triisocyanate is HDI trimer; the foaming agent is water or cyclopentane; the foam stabilizer is polyether silicone oil; and the leveling agent is one or more of BYK-322, BYK-333, and BYK-345.

4. The solvent-free polyurethane leather for automobile mats according to claim 1, characterized in that: The mass ratio of illite, diatomite and ferric chloride in step (1) is 20:10-30:5-10; the mass concentration of hydrochloric acid is 10-15%; the calcination temperature is 700-800°C and the calcination time is 3-5h; the concentration of barium chloride solution in step (2) is 0.1-0.5mol / L and the concentration of sodium sulfate solution is 0.1-0.5mol / L; the mass volume ratio of the mixed powder, barium chloride solution and sodium sulfate solution is 30g:200-400mL:200-400mL; and the stirring speed is 300-500r / min.

5. The solvent-free polyurethane leather for automobile mats according to claim 1, characterized in that: In step (3), the mass ratio of the modified particles, lanthanum oxide and polycarbosilane is 10-15:4-8:100; the temperature of the melt spinning is 280-320°C; the electron irradiation dose is 8-12MGy; the temperature of the high-temperature sintering is 1300-1500°C, and the sintering time is 3-6h; the temperature of the low-temperature crushing is below -50°C.

6. The solvent-free polyurethane leather for automobile mats according to claim 1, characterized in that: In step (4), the mass ratio of the inorganic particles / cross-linked silicon carbide fibers, phthalic anhydride, and zirconate coupling agent is 100:10-15:3-6; the stirring reaction temperature is 50-70°C, and the reaction time is 3-5h.

7. A method for preparing a solvent-free polyurethane leather for automobile mats as claimed in any one of claims 1 to 6, characterized in that: The following steps are involved: (a) weighing raw materials according to the formula, adding polyester polyol, polyether polyol, chain extender, foaming agent, foam stabilizer, leveling agent and catalyst into a reaction kettle, stirring and reacting to obtain component A; (b) adding diisocyanate, triisocyanate and radiation protection filler to component A of step (a), heating and reacting, cooling after the reaction is completed to obtain a slurry, and then coating the slurry on the surface of the release paper at a coating amount of 150-200 g / m2, and drying to form a polyurethane surface layer; (c) laminating the base fabric layer and the polyurethane surface layer in step (b) and pressing them together with a laminating roller. After lamination, the laminating process is completed and the laminating process is carried out in an oven for aging. After aging, the release paper is peeled off and the solvent-free polyurethane leather is obtained.

8. The preparation method according to claim 7, characterized in that: The stirring reaction temperature in step (a) is 60-90°C, the reaction time is 3-5h, and the stirring speed is 60-100r / min; the heating reaction temperature in step (b) is 70-90°C, the reaction time is 0.5-1h, and the drying conditions are 3-5min at 100-120°C; the laminating roller pressure in step (c) is 1-3MPa, and the oven aging conditions are 130-150°C oven aging for 8-12min.

9. A car mat, characterized in that: From top to bottom, it includes the solvent-free polyurethane leather layer as described in any one of claims 1 to 6, a high-density high-elastic foam layer, a non-woven fabric layer, a TPU hot-melt film layer, a TPU high-temperature resistant film layer, an adhesive resin layer, a high-gloss PET release film layer, and an environmentally friendly PP synthetic paper layer; Wherein, the high-density and high-elastic foam layer is electron irradiated cross-linked polyethylene foam with a density of 0.1-0.2 kg / cm3 and a thickness of 0.5-1 mm; the thickness of the non-woven fabric layer is 0.1-0.2 mm.