A method for producing hydrogen by coupling reforming of metal or metal hydride and methanol steam

By compounding the catalyst with metal or metal hydride and contacting it with methanol and water in the reactor, the problems of high raw material cost, large heat release and low hydrogen purity are solved, and efficient and low-cost hydrogen generation and The device is miniaturized.

CN115947304BActive Publication Date: 2024-10-22PEKING UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211671039.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-26
Publication Date
2024-10-22
Estimated Expiration
2042-12-26

AI Technical Summary

Technical Problem

In the existing technology, the cost of raw materials for hydrogen production through hydrolysis of metal or metal hydride is high and the amount of heat released is large. Methanol steam reforming requires heat absorption and the purity of hydrogen is low. It is difficult to miniaturize the hydrogen production device.

Method used

The catalyst used for methanol steam reforming is compounded with a metal or metal hydride capable of hydrolysis reaction to form an A-B compound, and is brought into contact with the mixture of methanol and water in the reactor, and the temperature and pressure are controlled to promote the reaction. , produces high-purity hydrogen and absorbs CO2 through metal or metal hydride hydrolysis products, reducing equipment requirements.

Benefits of technology

It achieves the generation of high-purity hydrogen, reduces equipment costs and heat loads, avoids additional heating requirements, and makes the device easier to miniaturize.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115947304B_ABST
    Figure CN115947304B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for producing hydrogen by coupling metal or metal hydride and methanol steam reforming, comprising the following steps: compounding a catalyst A for producing hydrogen by mixed steam reforming of methanol and water with a metal or metal hydride B capable of undergoing a hydrolysis reaction to obtain an A-B complex; loading the A-B complex into a reactor, adding a mixture of methanol and water, controlling the temperature and pressure in the reactor, leading the generated hydrogen out of the reactor, and stopping heating the reactor after a set reaction time. The byproduct CO2 generated during the methanol steam reforming process in the coupled reaction can be absorbed by the hydroxide generated by the hydrolysis of the metal or metal hydride, promoting the forward movement of the methanol reforming and water vapor conversion reactions, and having a higher hydrogen purity; in addition, the heat released by the hydrolysis of the metal or metal hydride in the coupled reaction can be supplied to the methanol reforming, without the need for additional heat.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of hydrogen storage, and in particular to a method for producing hydrogen by coupling reforming of metal or metal hydride with methanol steam. Background Art

[0002] High-performance hydrogen storage technology is the key to improving the endurance of hydrogen fuel cells. The current high-pressure gas cylinder hydrogen storage technology has disadvantages such as low hydrogen storage density, poor safety, and difficulty in refueling, which cannot meet the actual application needs, especially for special applications such as portable power supplies and drones. There is no need and conditions for hydrogen refueling at hydrogen refueling stations. It is urgent to develop efficient hydrogen supply technology with high hydrogen storage density, high hydrogen purity, and no reliance on hydrogen refueling infrastructure.

[0003] Hydrolysis of metals or metal hydrides and methanol steam reforming are two typical hydrogen production technologies. Hydrolysis of metals or metal hydrides produces high purity hydrogen, the reaction can proceed quickly and spontaneously, the hydrogen production device is simple, and it is easy to integrate into an efficient and compact portable hydrogen supply system, but the raw material cost is high and the hydrolysis heat release is large. Methanol can be produced by steam reforming, which has the advantages of high hydrogen storage density, easy transportation, and wide sources; but the methanol steam reforming process is an endothermic reaction, which requires a heating device. The main products of the reaction are H2, CO2 and a small amount of CO by-products, which need to be separated and purified before they can be supplied to fuel cells, which makes the equipment for methanol reforming complex and difficult to miniaturize. In recent years, researchers have also proposed a method for absorbing the CO2 produced by reforming through an absorbent. For example, in patent CN110694624A, a method for enhanced methanol steam reforming based on MgO-based absorbent is disclosed. MgO is used to absorb the CO2 produced during the reforming process, which promotes the forward movement of the reforming reaction and the water vapor shift reaction, reduces the concentration of CO and CO2 in the product, and improves the purity of hydrogen. However, the introduction of adsorbents will significantly reduce the hydrogen storage density of the entire system.

[0004] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention

[0005] The object of the present invention is to provide a method for producing hydrogen by coupling reforming of metal or metal hydride and methanol steam, which can solve the problems of high cost and high heat release of hydrolysis raw materials.

[0006] Another object of the present invention is to solve the problems that methanol steam reforming requires heat absorption, hydrogen purity is low, and hydrogen production equipment is difficult to miniaturize.

[0007] To achieve the above object, the present invention provides a method for producing hydrogen by coupling reforming of metal or metal hydride and methanol steam, comprising the following steps:

[0008] (1) Compounding a catalyst A used for hydrogen production by mixed steam reforming of methanol and water with a metal or metal hydride B capable of undergoing a hydrolysis reaction to obtain an AB complex;

[0009] (2) loading the AB complex obtained in step (1) into a reactor;

[0010] (3) adding a mixture of methanol and water into the reactor, controlling the temperature and pressure in the reactor, so that the mixture of methanol and water contacts and reacts with the AB complex;

[0011] (4) The generated hydrogen is led out of the reactor, and after a set reaction time, the heating of the reactor is stopped.

[0012] Preferably, the catalyst A used for hydrogen production by steam reforming of methanol and water in step (1) is a metal, alloy, oxide, halide, oxygen-containing acid salt or metal organic compound containing the metal element Mn, Fe, Co, Ni, Cu, Zn, Ru, Pd or Pt.

[0013] Preferably, in step (1), the catalyst A and the metal or metal hydride B are compounded by solid mechanical mixing such as grinding, ball milling or stirring.

[0014] Furthermore, in step (1), the catalyst A and the metal or metal hydride B are compounded in the following manner: the catalyst A component is dissolved in a solvent that does not react with the metal or metal hydride B to prepare a solution, the metal or metal hydride B is immersed in the solution containing the catalyst A, and then the solvent is removed.

[0015] Preferably, in step (1), the mass percentage of the catalyst A in the AB complex is 0.01%-50%.

[0016] Furthermore, in step (3), a mixture of methanol and water is added into the reactor, but the AB complex does not contact the mixture of methanol and water. Then, the reactor is heated to vaporize the mixture of methanol and water into mixed steam, and the mixed steam contacts and reacts with the AB complex.

[0017] Furthermore, in step (3), after the reactor is heated to a set temperature, a mixture of methanol and water is added to the reactor, and the mixture of methanol and water or mixed steam is injected into the reactor quantitatively or at a constant speed using a syringe or a pump.

[0018] Preferably, in step (3), the temperature and pressure in the reactor are controlled by a PID control system, the temperature in the reactor is controlled between 50-350° C., and the pressure is controlled between 0.1 Pa-20 MPa.

[0019] Furthermore, in step (4), the generated hydrogen is controlled by a pressure reducing valve or a mass flow controller of a gas path device to control the output pressure and gas flow rate.

[0020] Preferably, in step (4), whether the metal or hydride B is completely converted into carbonate is determined by the total amount of input gas and the total amount of generated gas.

[0021] Compared with the prior art, the method for producing hydrogen by coupling reforming of metal or metal hydride and methanol steam according to the present invention has the following beneficial effects:

[0022] 1. Compared with traditional methanol steam reforming hydrogen production, the by-product CO2 produced in the methanol steam reforming process in the coupled reaction can be absorbed by the hydroxide produced by the hydrolysis of metals or metal hydrides, promoting the forward movement of methanol reforming and water gas shift reactions, and has higher hydrogen purity, so no additional gas separation equipment or absorbent is required; in addition, the heat released by the hydrolysis of metals or metal hydrides in the coupled reaction can be supplied to methanol steam reforming, and no additional heat is required, which reduces equipment costs and solves the problem of difficulty in miniaturization of hydrogen production equipment.

[0023] 2. Compared with traditional hydrolysis hydrogen production, more hydrogen is produced per unit of metal or metal hydride, and the heat released per unit of hydrogen is lower, which greatly reduces the cost and the heat load of the hydrogen release system. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 is an X-ray diffraction pattern of the CuO / CaH2 composite in Example 1 of the present invention;

[0025] Figure 2 is a microscopic morphology image of the CuO / CaH2 composite taken by scanning electron microscope according to Example 1 of the present invention;

[0026] Figure 3 is an X-ray diffraction spectrum of a product after the CuO / CaH2 complex in Example 1 of the present invention reacts with a mixture of methanol and water;

[0027] Figure 4 This is a microscopic morphology of the product after the CuO / CaH2 complex reacts with a mixture of methanol and water, taken by scanning electron microscope according to Example 1 of the present invention. DETAILED DESCRIPTION

[0028] The specific implementation modes of the present invention are described in detail below in conjunction with the accompanying drawings, but it should be understood that the protection scope of the present invention is not limited by the specific implementation modes.

[0029] Unless explicitly stated otherwise, throughout the specification and claims, the term “comprise” or variations such as “include” or “comprising”, etc., will be understood to include the stated elements or components but not to exclude other elements or components.

[0030] According to the method for producing hydrogen by coupling metal or metal hydride and methanol steam reforming of the preferred embodiment of the present invention, the catalyst for producing hydrogen by methanol steam reforming is compounded with a metal or metal hydride capable of undergoing a hydrolysis reaction to obtain a composite, and then a mixed vapor of methanol and water is added to contact and react with the composite to produce hydrogen. The byproduct CO2 produced in the methanol steam reforming process in the coupling reaction can be absorbed by the hydroxide produced by the hydrolysis of the metal or metal hydride, promoting the forward movement of the methanol reforming and water vapor conversion reactions, and having a higher hydrogen purity.

[0031] A method for producing hydrogen by coupling reforming of metal or metal hydride with methanol steam comprises the following steps:

[0032] (1) A catalyst A used for hydrogen production by mixed steam reforming of methanol and water is compounded with a metal or metal hydride B capable of undergoing a hydrolysis reaction to obtain an AB complex.

[0033] The catalyst A used for hydrogen production by methanol and steam reforming is a metal, alloy, oxide, halide, oxyacid salt or metal organic compound containing metal elements such as Mn, Fe, Co, Ni, Cu, Zn, Ru, Pd or Pt. The catalyst A and the metal or metal hydride B can be compounded by: solid mechanical mixing, such as grinding, ball milling, stirring, etc.; or, the A component is dissolved in a solvent that does not react with B to prepare a solution, B is immersed in the solution containing A, and then the solvent is removed. The mass percentage of catalyst A in the AB complex is 0.01%-50%.

[0034] (2) Load the AB complex into the reactor.

[0035] The reactor can be selected from any shape.

[0036] (3) Introducing a mixture of methanol and water into the reactor, controlling the temperature and pressure in the reactor, so that the mixture contacts and reacts with the AB complex in the reactor.

[0037] Introducing a mixture of methanol and water into a reactor includes the following methods: (a) placing a mixed solution of methanol and water into a reactor together with an AB complex without contacting each other, and heating the reactor to vaporize the methanol and water and react with the AB complex; (b) heating the reactor to a set temperature, and injecting a certain amount of a mixed solution of methanol and water or mixed steam into the reactor using a syringe or a pump; (c) heating the reactor to a set temperature, and then gradually introducing a mixed solution of methanol and water at a certain rate using a peristaltic pump, an injection pump or other equipment, or introducing a mixed steam of methanol and water at a certain rate using a mass flow meter.

[0038] The temperature and pressure in the reactor are controlled by a PID control system, wherein the temperature is controlled between 50-350°C and the pressure is controlled between 0.1Pa-20MPa.

[0039] (4) The generated hydrogen is led out of the reactor.

[0040] The generated hydrogen can be controlled by common gas path devices such as pressure reducing valves and mass flow controllers to control the output pressure and gas flow rate.

[0041] (5) After the set reaction time, stop heating the reactor. If the mixture of methanol and water is introduced into the reactor in the form of (c) in step (3), stop heating the reactor and stop inputting the mixed steam of methanol and water into the reactor. When the temperature of the heater drops to room temperature, analyze the substances in the reactor.

[0042] Example 1

[0043] Take 0.2g CuO powder and 2g CaH2 powder, mix them in a ball mill filled with argon at a ball-to-material ratio of 20:1 and a rotation speed of 150rpm for 15min to obtain a CuO / CaH2 composite. Figure 1 As shown, the CuO / CaH2 complex is subjected to X-ray diffraction analysis to obtain an X-ray diffraction pattern of the CuO / CaH2 complex; as shown Figure 2As shown, the microscopic morphology of the CuO / CaH2 complex was taken by scanning electron microscope, and the magnification of the scanning electron microscope was 2000 times. Take 1.0g of the above CuO / CaH2 complex and put it in a reactor. Put 1.0mL H2O and 0.4mL CH3OH in a crucible and put them in the reactor at the same time to separate them from the solid complex. Evacuate the reactor to 1Pa, heat it to 250℃ at 20℃ / min, and react for 3h. After the reaction, the pressure in the reactor is 5.6MPa. Cool it to room temperature, and quantify the gas produced in the reactor with a mass flowmeter through a pressure reducing valve. The total volume of the gas produced is 1845mL (under standard conditions). After chromatographic quantification, it is found that the purity of hydrogen exceeds 99.9%, and the concentrations of CO2 and CO are both lower than the chromatographic detection limit. Figure 3 As shown, the solid produced after the reaction was subjected to X-ray diffraction analysis, and the product was mainly CaCO3, indicating that the Ca(OH)2 produced by hydrolysis reacted with the CO2 produced by methanol reforming. The overall reaction is as follows:

[0044] CaH2+CH3OH+2H2O=CaCO3+5H2

[0045] like Figure 4 As shown, the product produced after the reaction was photographed using a scanning electron microscope. The magnification of the scanning electron microscope was 2000 times, and a microscopic morphology of the product was obtained.

[0046] The gas produced by this scheme is only hydrogen, and it is an exothermic reaction that can proceed spontaneously. Compared with the traditional method of coupling hydrogen production by methanol steam reforming, it has the advantages of high hydrogen purity and no need for additional heat. The advantage of this scheme compared to CaH2 hydrolysis is that it has a higher hydrogen storage density. The reactants of this system include 1.0gCuO / CaH2 complex, 1.0mLH2O (1.0g) and 0.4mL CH3OH (0.32g), with a total mass of 2.32g; the generated hydrogen is 1845mL (under standard conditions), with a mass of 1845 / 11200=0.165g, and the hydrogen storage density reaches 7.1%.

[0047] The hydrolysis reaction of CaH2 proceeds according to the following equation:

[0048] CaH2+2H2O=Ca(OH)2+2H2

[0049] The reactants contain 1 mol CaH2 and 2 mol H2O, producing 2 mol H2, whose theoretical hydrogen storage density is only 5.13%.

[0050] Example 2

[0051] Take 0.2g CuCl powder and 2g CaH2 powder, mix them in a ball mill filled with argon at a ball-to-material ratio of 20:1 and a rotation speed of 150rpm for 15min to obtain a CuCl / CaH2 complex. Take 0.92g of the above CuCl / CaH2 complex and place it in a reactor with a liquid inlet. The reactor is evacuated to 1Pa, heated to 200℃ at 20℃ / min, the liquid inlet is opened, and a mixed solution of 1.0mL H2O and 0.3mL CH3OH is injected into the reactor by a syringe. The liquid inlet is closed and the reaction is carried out at this temperature for 5h. After the reaction, the pressure in the reactor is 4.1MPa. The reactor is cooled to room temperature, and the gas generated in the reactor is quantified by a mass flowmeter through a pressure reducing valve. The total volume of the generated gas is 1480mL (under standard conditions). After chromatographic quantification, the purity of hydrogen is measured to be more than 99.9%, and the concentrations of CO2 and CO are both lower than the chromatographic detection limit. X-ray diffraction analysis of the solid produced after the reaction showed that the product was mainly CaCO3.

[0052] Example 3

[0053] Take 0.2g of acetylacetonate palladium (molecular formula is C 10 H 14 Pd / MgH2 was dissolved in 10 mL of anhydrous tetrahydrofuran, 5 g of MgH2 powder was fully ground in a mortar and immersed in the above-mentioned tetrahydrofuran solution of acetylacetonate palladium, and stirred at room temperature for 2 h. The tetrahydrofuran was removed under reduced pressure at room temperature, and the obtained solid composite was placed in a tube furnace. Under an argon flow, the temperature was raised at a controlled low speed from room temperature to 200 ° C at a rate of 2 ° C / min, and kept warm for 2 h. Under an argon flow, the temperature was lowered to room temperature at a rate of 2 ° C / min to obtain a Pd / MgH2 composite.

[0054] 4.0 g of the above Pd / MgH2 complex was placed in a stainless steel tube, quartz wool was plugged at both ends, the stainless steel tube was heated to 120°C, and a mixed steam of methanol and water was introduced into the quartz tube, the volume ratio of methanol to water in the steam was 1:6, the steam introduction rate was 0.2 mL / min, and the pressure in the stainless steel reactor was 0.2 MPa. The gas produced by the reaction was condensed and measured with a mass flow meter, and the total volume of the produced gas was 5310 mL (under standard conditions). The proportion of hydrogen in the produced gas was measured by gas chromatography to be 99.0%, the content of CO was 0.2%, and the concentration of CO2 was below the detection limit. The solid produced after the reaction was analyzed by X-ray diffraction, and the product was a mixture of Mg(OH)2 and MgCO3.

[0055] The foregoing description of specific exemplary embodiments of the present invention is for the purpose of illustration and demonstration. These descriptions are not intended to limit the present invention to the precise form disclosed, and it is clear that many changes and variations can be made based on the above teachings. The purpose of selecting and describing the exemplary embodiments is to explain the specific principles of the present invention and its practical application, so that those skilled in the art can realize and utilize various different exemplary embodiments of the present invention and various different selections and changes. The scope of the present invention is intended to be limited by the claims and their equivalents.

Claims

1. A method for producing hydrogen by coupling reforming of metal or metal hydride with methanol steam, It is characterized in that The following steps are involved: (1) Compounding a catalyst A used for hydrogen production by mixed steam reforming of methanol and water with a metal or metal hydride B capable of undergoing a hydrolysis reaction to obtain an AB complex; (2) loading the AB complex obtained in step (1) into a reactor; (3) adding a mixture of methanol and water into the reactor, controlling the temperature and pressure in the reactor, so that the mixture of methanol and water contacts and reacts with the AB complex; (4) The generated hydrogen is led out of the reactor, and after a set reaction time, the heating of the reactor is stopped.

2. The method for producing hydrogen by coupling reforming of metal or metal hydride and methanol steam as claimed in claim 1, It is characterized in that The catalyst A used for hydrogen production by steam reforming of methanol and water in step (1) is one of metals, alloys, oxides, halides, oxygen-containing acid salts or metal organic compounds containing the metal elements Mn, Fe, Co, Ni, Cu, Zn, Ru, Pd or Pt.

3. The method for producing hydrogen by coupling reforming of metal or metal hydride and methanol steam as claimed in claim 1, It is characterized in that In step (1), the catalyst A and the metal or metal hydride B are compounded by solid mechanical mixing such as grinding, ball milling or stirring.

4. The method for producing hydrogen by coupling reforming of metal or metal hydride and methanol steam as claimed in claim 1, It is characterized in that In step (1), the catalyst A and the metal or metal hydride B are compounded in the following manner: the catalyst A component is dissolved in a solvent that does not react with the metal or metal hydride B to prepare a solution, the metal or metal hydride B is immersed in the solution containing the catalyst A, and then the solvent is removed.

5. The method for producing hydrogen by coupling reforming of metal or metal hydride and methanol steam as claimed in claim 1, It is characterized in that In step (1), the mass percentage of the catalyst A in the AB complex is 0.01%-50%.

6. The method for producing hydrogen by coupling reforming of metal or metal hydride and methanol steam as claimed in claim 1, It is characterized in that In step (3), a mixture of methanol and water is added to the reactor, but the AB complex does not contact the mixture of methanol and water. The reactor is then heated to vaporize the mixture of methanol and water into mixed steam, and the mixed steam contacts and reacts with the AB complex.

7. The method for producing hydrogen by coupling reforming of metal or metal hydride and methanol steam as claimed in claim 1, It is characterized in that In step (3), after the reactor is heated to a set temperature, a mixture of methanol and water is added to the reactor, and the mixture of methanol and water or mixed steam is injected into the reactor quantitatively or at a constant speed using a syringe or a pump.

8. The method for producing hydrogen by coupling reforming of metal or metal hydride and methanol steam as claimed in claim 1, It is characterized in that In step (3), the temperature and pressure in the reactor are controlled by a PID control system, the temperature in the reactor is controlled between 50-350° C., and the pressure is controlled between 0.1 Pa-20 MPa.

9. The method for producing hydrogen by coupling reforming of metal or metal hydride and methanol steam as claimed in claim 1, It is characterized in that In step (4), the generated hydrogen is controlled by a pressure reducing valve or a mass flow controller of a gas path device to output pressure and gas flow rate.

10. The method for producing hydrogen by coupling reforming of metal or metal hydride and methanol steam as claimed in claim 1, It is characterized in that In step (4), whether the metal or hydride B is completely converted into carbonate is determined by the total amount of input gas and the total amount of generated gas.