A nitrogen-doped molybdenum carbide and carbon composite nanomaterial and preparation method thereof

A method using molybdenum-containing salts and soybean meal in a planetary ball mill addresses the challenges of existing molybdenum carbide production, enabling cost-effective and scalable production of nitrogen-doped molybdenum carbide and carbon composite nanomaterials with enhanced properties.

CN115947342BActive Publication Date: 2024-12-06LULIANG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310015773.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-04
Publication Date
2024-12-06
Estimated Expiration
2043-01-04

AI Technical Summary

Technical Problem

Existing methods for preparing molybdenum carbide nanostructures face challenges such as the need for hazardous gases, expensive equipment, high parameter control accuracy, harsh conditions, low yields, and material agglomeration, making large-scale production difficult.

Method used

A method involving the use of molybdenum-containing salts and soybean meal in a planetary ball mill, followed by high-temperature reduction carbonization and passivation, without requiring flammable gases or complex instruments, to produce nitrogen-doped molybdenum carbide and carbon composite nanomaterials.

Benefits of technology

The method is cost-effective, safe, and scalable, producing materials suitable for industrial applications with improved stability and activity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115947342B_ABST
    Figure CN115947342B_ABST
Patent Text Reader

Abstract

The present invention provides a nitrogen-doped molybdenum carbide and carbon composite nanomaterial and a preparation method thereof. Specifically, a molybdenum-containing salt is used as a molybdenum source, and soybean meal is used as a chelating agent and a carbon source. The mixture is mechanically mixed and ground by a simple planetary ball mill to obtain a mixture precursor. The mixture precursor is then heated under an inert atmosphere, subjected to an in-situ high-temperature reduction carbonization treatment, and then cooled to room temperature. The mixture is passivated at room temperature to obtain a nitrogen-doped molybdenum carbide and carbon composite nanomaterial. In the synthesis process of the preparation method of the present invention, molybdenum-containing salt and waste biomass soybean meal are used as raw materials, which are widely available and inexpensive. The preparation method is simple, the process route is short, and no complex and precise instruments are required. No flammable and explosive gases are required. The material is safe and pollution-free, and the controllability is strong, which is conducive to large-scale industrial applications. The nitrogen-doped molybdenum carbide and carbon composite nanomaterial prepared by the present invention has good application prospects in the fields of catalysis, supercapacitors, and batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nano material preparation methods, and specifically relates to a nitrogen-doped molybdenum carbide and carbon composite nano material and a preparation method thereof. Background Art

[0002] In recent years, nano-functional materials have become a research hotspot due to their unique properties due to their own structure and characteristics, which make them have better optical, electrical, thermal, magnetic, mechanical and catalytic properties than bulk materials. Molybdenum carbide has been widely reported as an advanced energy material in the fields of catalysis, supercapacitors and batteries due to its unique physical and chemical properties.

[0003] The traditional method of preparing molybdenum carbide is to directly carbonize molybdenum at high temperature (1500~2300ºC). Although the process is simple and effective and suitable for industrial production, the material activity is very poor. With the advancement of preparation technology, many methods have been used to prepare molybdenum carbide nanostructures, mainly including programmed temperature reaction, carbon thermal hydrogen reduction, chemical vapor deposition, solvothermal method and microwave-assisted preparation. However, the above preparation methods either require the introduction of reducing hazardous gases such as CO, H 2 , CH 4 Or other hydrocarbons, either require sophisticated and expensive equipment, and the preparation process requires extremely high parameter control accuracy, harsh conditions, high costs, and low yields, making it difficult to achieve large-scale production.

[0004] In addition, since nanostructured molybdenum carbide itself has the problem of high specific surface energy, it is very easy to agglomerate during the preparation process, causing a serious decrease in the activity of the material.

[0005] Based on this, a method for preparing nitrogen-doped molybdenum carbide and carbon composite nanomaterials was proposed. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a method for preparing nitrogen-doped molybdenum carbide and carbon composite nanomaterials in view of the deficiencies of the above-mentioned prior art, so as to solve the problems raised in the above-mentioned background technology.

[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for preparing nitrogen-doped molybdenum carbide and carbon composite nanomaterials, comprising the following steps:

[0008] S1, adding molybdenum-containing salt and soybean meal into a planetary ball mill in proportion, and grinding to obtain a mixture precursor;

[0009] S2: The mixture precursor is heated in an inert atmosphere to perform an in-situ high-temperature reduction carbonization treatment, and then cooled to room temperature and passivated at room temperature to obtain nitrogen-doped molybdenum carbide and carbon composite nanomaterials.

[0010] Furthermore, in S1, the mass ratio of the molybdenum-containing salt to the soybean meal is 3.5:1 to 0.5:1.

[0011] Furthermore, in S1, the molybdenum-containing salt is specifically at least one of ammonium molybdate, molybdenum chloride, molybdenum acetate, sodium molybdate and potassium molybdate.

[0012] Furthermore, in S1, the grinding speed of the planetary ball mill is 100 to 600 rpm, and the grinding time is 30 to 300 min.

[0013] Furthermore, in S2, the inert atmosphere is at least one of nitrogen and argon.

[0014] Furthermore, in S2, the process parameters of the in-situ high-temperature reduction carbonization treatment are: temperature 650-950°C, holding time 0.5-6h, and heating rate 1-10°C / min.

[0015] Further, in S2, the process parameters of the passivation treatment are: at a volume ratio of 1% O 2 / Passivate in Ar atmosphere for 6~24h.

[0016] The present invention also provides a nitrogen-doped molybdenum carbide and carbon composite nanomaterial prepared by the above preparation method.

[0017] Compared with the prior art, the present invention has the following advantages:

[0018] The preparation method of nitrogen-doped molybdenum carbide and carbon composite nanomaterial provided by the present invention adopts molybdenum-containing salt and waste biomass soybean meal as raw materials, which are widely available and low in price, and has a simple preparation process and a short process route, does not require complex and precise instruments, does not require flammable and explosive gases, is safe and pollution-free, has strong controllability, and is conducive to large-scale industrial applications.

[0019] The nitrogen-doped molybdenum carbide and carbon composite nanomaterial prepared by the present invention will have broad application prospects in the fields of catalysis, supercapacitors and batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a scanning electron microscope (SEM) photograph of the nitrogen-doped molybdenum carbide and carbon composite nanomaterial obtained in Example 1 of the present invention.

[0021] Figure 2 This is an X-ray diffraction XRD pattern of the nitrogen-doped molybdenum carbide and carbon composite nanomaterial obtained in Example 2 of the present invention.

[0022] Figure 3 This is a high-resolution transmission electron microscopy (HRTEM) image of the nitrogen-doped molybdenum carbide and carbon composite nanomaterial obtained in Example 3 of the present invention.

[0023] Figure 4 This is an X-ray diffraction XRD pattern of the nitrogen-doped molybdenum carbide and carbon composite nanomaterial obtained in Example 4 of the present invention. DETAILED DESCRIPTION

[0024] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] Embodiment 1, the present invention provides a technical solution: a method for preparing nitrogen-doped molybdenum carbide and carbon composite nanomaterials, comprising the following steps:

[0026] S1: 5.0 g of ammonium molybdate and 5.0 g of soybean meal powder were added into a planetary ball mill and ground at 200 rpm for 200 min to obtain a mixture precursor;

[0027] S2: The obtained precursor mixture was heated to 750°C at a rate of 10°C / min under an argon atmosphere and kept at this temperature for 2.0 h, cooled to room temperature, and heated in 1% by volume O 2 / Ar atmosphere for 12 hours to obtain nitrogen-doped molybdenum carbide and carbon composite nanomaterials. The scanning electron microscope (SEM) photos of the obtained nitrogen-doped molybdenum carbide and carbon composite nanomaterials are as follows: Figure 1 shown.

[0028] Embodiment 2, the present invention provides a technical solution: a method for preparing nitrogen-doped molybdenum carbide and carbon composite nanomaterials, comprising the following steps:

[0029] S1: 10.0 g of molybdenum acetate and 5.0 g of soybean meal were added into a planetary ball mill and ground at 600 rpm for 60 min to obtain a mixture precursor;

[0030] S2: The obtained precursor mixture was heated to 800°C at 5°C / min under an argon atmosphere and kept at this temperature for 2.0 h, cooled to room temperature, and heated in 1% by volume O 2 / Ar atmosphere for 6 hours to obtain nitrogen-doped molybdenum carbide and carbon composite nanomaterials. The X-ray diffraction XRD pattern of the obtained nitrogen-doped molybdenum carbide and carbon composite nanomaterials is as follows Figure 2 shown.

[0031] Embodiment 3, the present invention provides a technical solution: a method for preparing nitrogen-doped molybdenum carbide and carbon composite nanomaterials, comprising the following steps:

[0032] S1: 7.5 g potassium molybdate and 5.0 g soybean meal powder were added into a planetary ball mill and ground at 400 rpm for 300 min to obtain a mixture precursor;

[0033] S2: The obtained precursor mixture was heated to 900°C at a rate of 2°C / min under a nitrogen atmosphere and kept at this temperature for 1.0 h, cooled to room temperature, and heated in 1% by volume O 2 / Ar atmosphere for 18 hours to obtain nitrogen-doped molybdenum carbide and carbon composite nanomaterials. The high-resolution transmission electron microscopy HRTEM image of the obtained nitrogen-doped molybdenum carbide and carbon composite nanomaterials is as follows: Figure 3 shown.

[0034] Embodiment 4, the present invention provides a technical solution: a method for preparing nitrogen-doped molybdenum carbide and carbon composite nanomaterials, comprising the following steps:

[0035] S1: 2.5 g sodium molybdate and 5.0 g soybean meal powder were added into a planetary ball mill and ground at 300 rpm for 120 min to obtain a mixture precursor;

[0036] S2: The obtained precursor mixture was heated to 700 °C at 1 °C / min under an argon atmosphere and kept at this temperature for 6.0 h, cooled to room temperature, and heated in 1% by volume O 2 / Ar atmosphere for 24 hours to obtain nitrogen-doped molybdenum carbide and carbon composite nanomaterials. The X-ray photoelectron spectrum XPS graph of the obtained nitrogen-doped molybdenum carbide and carbon composite nanomaterials is as follows Figure 4 shown.

[0037] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0038] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing nitrogen-doped molybdenum carbide and carbon composite nanomaterials, characterized in that: The following steps are involved: S1. Adding molybdenum-containing salt and soybean meal into a planetary ball mill in proportion, grinding to obtain a mixture precursor; the mass ratio of the molybdenum-containing salt to the soybean meal is 3.5:1 to 0.5:1; S2: heating the mixture precursor under an inert atmosphere, performing an in-situ high-temperature reduction carbonization treatment, then cooling to room temperature, and passivating at room temperature to obtain nitrogen-doped molybdenum carbide and carbon composite nanomaterials; The process parameters of the in-situ high-temperature reduction carbonization treatment are: temperature 650-950°C, holding time 0.5-6h, heating rate 1-10°C / min; The process parameters of the passivation treatment are: passivation in an O2 / Ar atmosphere with a volume ratio of 1% for 6 to 24 hours.

2. The method for preparing a nitrogen-doped molybdenum carbide and carbon composite nanomaterial according to claim 1, characterized in that: In S1, the molybdenum-containing salt is specifically at least one of ammonium molybdate, molybdenum chloride, molybdenum acetate, sodium molybdate and potassium molybdate.

3. The method for preparing a nitrogen-doped molybdenum carbide and carbon composite nanomaterial according to claim 1, characterized in that: In S1, the grinding speed of the planetary ball mill is 100-600 rpm, and the grinding time is 30-300 min.

4. The method for preparing a nitrogen-doped molybdenum carbide and carbon composite nanomaterial according to claim 1, characterized in that: In S2, the inert atmosphere is at least one of nitrogen and argon.