Composition, laminate, and method for producing laminate

By using the compositions of compounds (A), (B) and (C), a substrate laminate with low thermal expansion rate and high bonding strength is formed, and warping of the adhesive caused by the difference in thermal expansion rate in the substrate lamination and the warping of the adhesive and the like in the substrate lamination are solved. The peeling problem achieves excellent bonding strength and reliability.

CN115956098BActive Publication Date: 2024-11-26MITSUI CHEMICALS INC
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202180050465.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-09-10
Filing Date
2021-09-08
Publication Date
2024-11-26
Estimated Expiration
2041-09-08

AI Technical Summary

Technical Problem

The existing adhesives have problems of warping and peeling due to differences in thermal expansion rates during substrate lamination. The addition of inorganic fillers reduces the bonding strength, making it difficult to take into account both low thermal expansion rates and high bonding strength.

Method used

Using a composition containing compound (A), compound (B) and compound (C), compound (A) has Si-O bonds and cationic functional groups, and compound (B) has a plurality of -C(=O)OX groups and -C(=O)OH group, compound (C) has a ring structure and a directly bound primary nitrogen atom. The reaction products of these compounds form a laminate with low thermal expansion and high bonding strength.

Benefits of technology

The low thermal expansion rate and high bonding strength of the substrate laminate are achieved, the reliability and bonding strength of the laminate are improved, and the strain and peeling problems caused by the difference in thermal expansion rate are avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0004080316440000051
    Figure GDA0004080316440000051
  • Figure GDA0004080316440000061
    Figure GDA0004080316440000061
  • Figure GDA0004080316440000081
    Figure GDA0004080316440000081
Patent Text Reader

Abstract

The present invention provides a composition, which comprises a compound (A), a compound (B) and a compound (C), wherein the compound (A) has a cationic functional group comprising at least one selected from a primary nitrogen atom and a secondary nitrogen atom and a Si-O bond, the compound (B) has three or more -C(=O)OX groups (X is a hydrogen atom or an alkyl group having 1 to 6 carbon atoms), wherein one or more and six of the -C(=O)OX groups are -C(=O)OH groups, and the compound (C) has a ring structure and one or more primary nitrogen atoms directly bonded to the ring structure, and the ratio of the primary nitrogen atoms and secondary nitrogen atoms contained in the compound (A) to the total of the primary nitrogen atoms and secondary nitrogen atoms contained in the compound (A) and the primary nitrogen atoms contained in the compound (C) is 3 mol% to 95 mol%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a composition, a laminate, and a method for producing the laminate. Background Art

[0002] As electronic devices become smaller, lighter, and more powerful, they require semiconductor chips and the like to be highly integrated. However, it is difficult to fully meet this requirement by simply miniaturizing the circuit. Therefore, in recent years, a method has been proposed to achieve high integration by vertically stacking multiple substrates (wafers), semiconductor chips, and the like to form a multi-layer three-dimensional structure.

[0003] As a method for stacking substrates (wafers), chips, etc. (hereinafter, sometimes referred to as "substrates, etc."), there have been proposed methods of directly bonding substrates to each other (fusion bonding), methods of bonding substrates to each other using an adhesive, and the like.

[0004] For details of the above method, reference can be made to, for example, Japanese Patent Application Publication No. 4-132258, Japanese Patent Application Publication No. 2010-226060, Japanese Patent Application Publication No. 2016-47895, A. Bayrashev, B. Ziaie, Sensors and Actuators A 103 (2003) 16-22, and QY Tong, UM Gosele, Advanced Material 11, No. 17 (1999) 1409-1425. Summary of the invention

[0005] Problems to be solved by the invention

[0006] The method using an adhesive has the advantage of being able to bond substrates to each other at a lower temperature than fusion bonding, but may cause strain on the bonding surface due to the difference in thermal expansion coefficient between the adhesive and the substrate, resulting in warping and peeling. As a method for reducing the thermal expansion coefficient of the adhesive, adding an inorganic filler may be considered, but the bonding strength may be reduced due to the addition of an inorganic filler. Therefore, it is desirable to develop a material that can take into account both low thermal expansion coefficient and high bonding strength.

[0007] One embodiment of the present invention has been made in view of the above-mentioned problems, and an object of the present invention is to provide a composition having a low thermal expansion coefficient and excellent bonding strength with a substrate, a laminate obtained using the composition, and a method for producing a laminate using the composition.

[0008] Methods for solving problems

[0009] The specific means for solving the above-mentioned problems are as follows.

[0010] <1> A composition comprising a compound (A), a compound (B) and a compound (C),

[0011] The compound (A) has a cationic functional group including at least one selected from a primary nitrogen atom and a secondary nitrogen atom and a Si—O bond,

[0012] The compound (B) has 3 or more -C(=O)OX groups (X is a hydrogen atom or an alkyl group having 1 to 6 carbon atoms), and among the 3 or more -C(=O)OX groups, 1 to 6 are -C(=O)OH groups.

[0013] The compound (C) has a ring structure and one or more primary nitrogen atoms directly bonded to the ring structure,

[0014] The ratio of the primary nitrogen atoms and secondary nitrogen atoms contained in the compound (A) to the total of the primary nitrogen atoms and secondary nitrogen atoms contained in the compound (A) and the primary nitrogen atoms contained in the compound (C) is 3 mol % to 95 mol %.

[0015] <2> The composition according to <1>, wherein the compound (C) has two or more primary nitrogen atoms directly bonded to the ring structure.

[0016] <3> The composition according to <1> or <2>, wherein the weight average molecular weight of the compound (C) is 80 or more and 600 or less.

[0017] <4> The composition according to any one of <1> to <3>, wherein the compound (A) has two alkyl groups bonded to the oxygen atom constituting the Si—O bond.

[0018] <5> The composition according to any one of <1> to <4>, wherein the weight average molecular weight of the compound (B) is 200 or more and 600 or less.

[0019] <6> The composition according to any one of <1> to <5>, further comprising a polar solvent.

[0020] <7> The composition according to any one of <1> to <6>, which is used for producing a semiconductor device.

[0021] <8> The composition according to any one of <1> to <7>, which is used for forming a layer on a substrate or between substrates.

[0022] <9> A laminate comprising a layer and a substrate,

[0023] The layer comprises a reaction product of compound (A), compound (B) and compound (C),

[0024] The compound (A) has a cationic functional group including at least one selected from a primary nitrogen atom and a secondary nitrogen atom and a Si—O bond,

[0025] The compound (B) has 3 or more -C(=O)OX groups (X is a hydrogen atom or an alkyl group having 1 to 6 carbon atoms), and among the 3 or more -C(=O)OX groups, 1 to 6 are -C(=O)OH groups.

[0026] The compound (C) has a ring structure and one or more primary nitrogen atoms directly bonded to the ring structure,

[0027] The ratio of the primary nitrogen atoms and secondary nitrogen atoms contained in the compound (A) to the total of the primary nitrogen atoms and secondary nitrogen atoms contained in the compound (A) before the reaction and the primary nitrogen atoms contained in the compound (C) is 3 mol% to 95 mol%.

[0028] <10> The laminated body according to claim 9, wherein the substrate includes a first substrate and a second substrate, and the first substrate, the layer containing the reaction product, and the second substrate are arranged in this order.

[0029] <11> A method for producing a laminate, comprising: forming a layer on a substrate or between substrates; and curing the layer.

[0030] The layer comprises compound (A), compound (B) and compound (C),

[0031] The compound (A) has a cationic functional group including at least one selected from a primary nitrogen atom and a secondary nitrogen atom and a Si—O bond,

[0032] The compound (B) has 3 or more -C(=O)OX groups (X is a hydrogen atom or an alkyl group having 1 to 6 carbon atoms), and among the 3 or more -C(=O)OX groups, 1 to 6 are -C(=O)OH groups.

[0033] The compound (C) has a ring structure and one or more primary nitrogen atoms directly bonded to the ring structure,

[0034] The ratio of the primary nitrogen atoms and secondary nitrogen atoms contained in the compound (A) to the total of the primary nitrogen atoms and secondary nitrogen atoms contained in the compound (A) and the primary nitrogen atoms contained in the compound (C) is 3 mol % to 95 mol %.

[0035] Effects of the Invention

[0036] According to one embodiment of the present invention, there are provided a composition having a low thermal expansion coefficient and excellent bonding strength with a substrate, a laminate obtained using the composition, and a method for producing a laminate using the composition. DETAILED DESCRIPTION

[0037] In the present disclosure, a numerical range expressed using "to" means a range including the numerical values ​​described before and after "to" as the lower limit and the upper limit.

[0038] In the numerical range of hierarchical recording in the present disclosure, the upper limit or lower limit of recording in a numerical range can be replaced by the upper limit or lower limit of the numerical range of other hierarchical recordings. In addition, in the numerical range of recording in the present disclosure, the upper limit or lower limit of the numerical range can also be replaced by the value shown in the embodiment.

[0039] <Composition>

[0040] The composition of the present embodiment is a composition comprising a compound (A), a compound (B) and a compound (C), wherein the compound (A) has a cationic functional group including at least one selected from a primary nitrogen atom and a secondary nitrogen atom and a Si-O bond, the compound (B) has three or more -C(=O)OX groups (X is a hydrogen atom or an alkyl group having 1 to 6 carbon atoms), of which one or more of the three or more -C(=O)OX groups are -C(=O)OH groups, and the compound (C) has a ring structure and one or more primary nitrogen atoms directly bonded to the ring structure, and the ratio of the primary nitrogen atoms and secondary nitrogen atoms contained in the compound (A) to the total of the primary nitrogen atoms and secondary nitrogen atoms contained in the compound (A) and the primary nitrogen atoms contained in the compound (C) is 3 mol% to 95 mol%.

[0041] The above-mentioned composition comprises compound (A) and compound (C) as 2 kinds of components reacting with compound (B). The present inventors have studied, and the result shows that the cured product obtained by using the composition has a lower thermal expansion coefficient than the cured product obtained by only using compound (A) as a component reacting with compound (B). Therefore, it is believed that in the laminate obtained by using the above-mentioned composition, the bonding surface of the layer formed by the composition and the substrate is not easy to be strained, and the reliability is excellent.

[0042] The layer obtained using the above composition is also excellent in bonding strength with the substrate.

[0043] (Compound (A))

[0044] Compound (A) has a cationic functional group including at least one of a primary nitrogen atom and a secondary nitrogen atom and a Si—O bond. The cationic functional group is not particularly limited as long as it is a functional group that can be positively charged and includes at least one of a primary nitrogen atom and a secondary nitrogen atom.

[0045] The cationic functional group containing at least one of the primary nitrogen atom and the secondary nitrogen atom contained in the compound (A) reacts with the carboxyl group of the compound (B) to form a cured product. The Si-O bond contained in the compound (A) contributes to improving the bonding strength with the substrate.

[0046] The compound (A) may be used alone or in combination of two or more.

[0047] Compound (A) may contain tertiary nitrogen atoms in addition to primary and secondary nitrogen atoms.

[0048] In the present disclosure, the so-called "primary nitrogen atom" refers to a nitrogen atom that is bonded only to two hydrogen atoms and one atom other than hydrogen atoms (for example, a nitrogen atom contained in a primary amino group (-NH2 group)), or a nitrogen atom that is bonded only to three hydrogen atoms and one atom other than hydrogen atoms (cation).

[0049] The so-called "secondary nitrogen atom" refers to a nitrogen atom that is bonded to only one hydrogen atom and two atoms other than a hydrogen atom (i.e., a nitrogen atom contained in the functional group represented by the following formula (a)), or a nitrogen atom that is bonded to only two hydrogen atoms and two atoms other than a hydrogen atom (cation).

[0050] The so-called "tertiary nitrogen atom" refers to a nitrogen atom bonded to only three atoms other than hydrogen atoms (i.e., a nitrogen atom as a functional group represented by the following formula (b)) or a nitrogen atom bonded to only one hydrogen atom and three atoms other than hydrogen atoms (cation).

[0051] [Chemistry 1]

[0052]

[0053] In formula (a) and formula (b), * represents a bonding position to an atom other than a hydrogen atom.

[0054] The functional group represented by the formula (a) may be a secondary amino group (-NHR a Here, R a The functional group representing a part of an alkyl group may be a divalent linking group contained in the polymer skeleton.

[0055] The functional group (ie, tertiary nitrogen atom) represented by the formula (b) may be a tertiary amino group (-NR b R c Here, R b and R c The functional groups each independently represent a part of an alkyl group) may be a trivalent linking group contained in the polymer skeleton.

[0056] From the viewpoint of reducing the water absorption of the cured product and reducing the amount of outgassing, the compound (A) preferably has two alkyl groups bonded to the oxygen atoms constituting the Si-O bond, and more preferably has alkyl groups bonded to two oxygen atoms bonded to one silicon atom constituting the Si-O bond, respectively. The number of carbon atoms of the two alkyl groups is preferably 1 to 5, more preferably 1 or 2, and further preferably 2, each independently.

[0057] The weight average molecular weight of the compound (A) is not particularly limited and may be, for example, 130 to 10,000, 130 to 5,000, or 130 to 2,000.

[0058] In the present disclosure, the weight average molecular weight of a compound refers to a weight average molecular weight in terms of polyethylene glycol measured by GPC (Gel Permeation Chromatography).

[0059] Specifically, the weight-average molecular weight is calculated using an aqueous solution of sodium nitrate at a concentration of 0.1 mol / L as a developing solvent, an analytical device Shodex DET RI-101 and two analytical columns (TSKgel G6000PWXL-CP and TSKgel G3000PWXL-CP manufactured by Tosoh), and the refractive index is detected at a flow rate of 1.0 mL / min. Polyethylene glycol / polyethylene oxide is used as a standard and calculated using analytical software (Empower 3 manufactured by Waters).

[0060] The compound (A) may further have an anionic functional group, a nonionic functional group, or the like as necessary.

[0061] The nonionic functional group may be a hydrogen bond accepting group or a hydrogen bond donating group. Examples of the nonionic functional group include a hydroxyl group, a carbonyl group, and an ether group (—O—).

[0062] The anionic functional group is not particularly limited as long as it is a functional group capable of carrying a negative charge. Examples of the anionic functional group include a carboxylic acid group, a sulfonic acid group, and a sulfate group.

[0063] Specific examples of the compound (A) include compounds having a Si-O bond and an amino group. Examples of the compound having a Si-O bond and an amino group include siloxane diamine, a silane coupling agent having an amino group, and a siloxane polymer of a silane coupling agent having an amino group.

[0064] As a silane coupling agent which has an amino group, the compound represented by following formula (A-3) is mentioned, for example.

[0065] [Chemistry 2]

[0066]

[0067] In formula (A-3), R 1 represents an alkyl group having 1 to 4 carbon atoms which may be substituted. 2 and R 3 Each independently represents an alkylene group having 1 to 12 carbon atoms, an ether group or a carbonyl group which may be substituted (a carbonyl group, an ether group or the like may be contained in the skeleton). 4 and R 5 Each independently represents an alkylene group having 1 to 4 carbon atoms which may be substituted or a single bond. Ar represents a divalent or trivalent aromatic ring. 1 represents hydrogen or an optionally substituted alkyl group having 1 to 5 carbon atoms. 2 represents hydrogen, a cycloalkyl group, a heterocyclic group, an aryl group, or an alkyl group having 1 to 5 carbon atoms which may be substituted (a carbonyl group, an ether group, etc. may be included in the skeleton). 1 , R 2 , R 3 , R 4 , R 5 , X 1 Can be the same or different.

[0068] As R 1 , R 2 , R 3 , R 4 , R 5 , X 1 , X 2 The substituents of the alkyl group and the alkylene group in the above-mentioned group are each independently amino, hydroxyl, alkoxy, cyano, carboxylic acid, sulfonic acid, halogen and the like.

[0069] Examples of the divalent or trivalent aromatic ring in Ar include a divalent or trivalent benzene ring. 2 Examples of the aryl group include a phenyl group, a methylbenzyl group, and a vinylbenzyl group.

[0070] Specific examples of the silane coupling agent represented by formula (A-3) include N-(2-aminoethyl)-3-aminopropylmethyldiethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminoisobutyldimethylmethoxysilane, N-(2-aminoethyl)-3-aminoisobutylmethyldimethoxysilane, N-(2-aminoethyl)-11-aminoundecyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, (aminoethylaminoethyl)phenyltriethoxysilane, methylbenzylaminoethylaminopropyltrimethoxysilane, benzylaminoethylaminopropyltriethoxysilane, 3-ureidopropyltriethoxysilane, Silane, (aminoethylaminoethyl)phenethyltrimethoxysilane, (aminoethylaminomethyl)phenethyltrimethoxysilane, N-[2-[3-(trimethoxysilyl)propylamino]ethyl]ethylenediamine, 3-aminopropyldiethoxymethylsilane, 3-aminopropyldimethoxymethylsilane, 3-aminopropyldimethylethoxysilane, 3-aminopropyldimethylmethoxysilane, trimethoxy[2-(2-aminoethyl)-3-aminopropyl]silane, diaminomethylmethyldiethoxysilane, methylaminomethylmethyldiethoxysilane, p-aminophenyltrimethoxysilane, N-methylaminopropyltriethoxysilane, N-methylaminopropylmethyldiethoxysilane, (phenylaminomethyl)methyldiethoxysilane, acetamidopropyltrimethoxysilane and hydrolyzates thereof.

[0071] Examples of amino group-containing silane coupling agents other than those represented by formula (A-3) include N,N-bis[3-(trimethoxysilyl)propyl]ethylenediamine, N,N'-bis[3-(trimethoxysilyl)propyl]ethylenediamine, bis[(3-triethoxysilyl)propyl]amine, piperazinylpropylmethyldimethoxysilane, bis[3-(triethoxysilyl)propyl]urea, bis(methyldiethoxysilylpropyl)amine, 2,2-dimethoxy-1,6-diaza-2-silacyclooctane, 3,5-diamino-N-(4-(methoxydimethylsilyl)phenyl)benzamide, 3,5-diamino-N-(4-(triethoxysilyl)phenyl)benzamide, 5-(ethoxydimethylsilyl)benzene-1,3-diamine, and hydrolyzates thereof.

[0072] The silane coupling agent having an amino group may be used alone or in combination of two or more.

[0073] In addition, polymers (siloxane polymers) formed by these silane coupling agents via siloxane bonds (Si-O-Si) can also be used. For example, polymers having a linear siloxane structure, polymers having a branched siloxane structure, polymers having a cyclic siloxane structure, polymers having a caged siloxane structure, etc. can be obtained from the hydrolyzate of 3-aminopropyltrimethoxysilane. The caged siloxane structure is represented by the following formula (A-1), for example.

[0074] [Chemistry 3]

[0075]

[0076] Examples of the siloxane diamine include compounds represented by the following formula (A-2): In the formula (A-2), i is an integer of 0 to 4, j is an integer of 1 to 3, and Me is a methyl group.

[0077] [Chemistry 4]

[0078]

[0079] Examples of the siloxane diamine include 1,3-bis(3-aminopropyl)tetramethyldisiloxane (in the formula (A-2), i=0, j=1) and 1,3-bis(2-aminoethylamino)propyltetramethyldisiloxane (in the formula (A-2), i=1, j=1).

[0080] Compound (A) has a cationic functional group including at least one of a primary nitrogen atom and a secondary nitrogen atom, and therefore can firmly bond substrates to each other through electrostatic interaction with functional groups such as hydroxyl, epoxy, carboxyl, amino, and mercapto groups that may be present on the surface of the substrate, or by tightly forming covalent bonds with the functional groups.

[0081] In addition, compound (A) has a cationic functional group containing at least one of a primary nitrogen atom and a secondary nitrogen atom, and therefore has excellent solubility in polar solvents, and can form a smooth film having high affinity for a substrate having a hydrophilic surface such as silicon.

[0082] As compound (A), from the viewpoint of heat resistance, a compound having an amino group as a cationic functional group is preferred. Furthermore, from the viewpoint of forming a thermally crosslinked structure such as amide, amideimide, or imide to further improve heat resistance, a compound having a primary amino group is preferred.

[0083] The ratio of the total number of primary and secondary nitrogen atoms to the number of silicon atoms in the compound (A) (total number of primary and secondary nitrogen atoms / number of silicon atoms) is not particularly limited, but is preferably 0.2 to 5 from the viewpoint of forming a smooth thin film.

[0084] The molar ratio of the Si element in the compound (A) to the non-crosslinking group such as a methyl group bonded to the Si element (non-crosslinking group / Si element) is preferably less than 2 (satisfying the relationship of non-crosslinking group / Si element < 2). It is believed that by satisfying this condition, the crosslinking density (crosslinking of Si-O-Si bonds with amide bonds, imide bonds, etc.) of the formed film is increased, and excellent bonding strength can be obtained.

[0085] As mentioned above, compound (A) has a cationic functional group containing at least one of a primary nitrogen atom and a secondary nitrogen atom. Here, when compound (A) contains a primary nitrogen atom, the proportion of primary nitrogen atoms in all nitrogen atoms in compound (A) is preferably 20 mol% or more, more preferably 25 mol% or more, and further preferably 30 mol% or more. In addition, compound (A) may have a cationic functional group containing a primary nitrogen atom and not containing a nitrogen atom other than a primary nitrogen atom (e.g., a secondary nitrogen atom, a tertiary nitrogen atom).

[0086] When the ratio of primary nitrogen atoms to all nitrogen atoms in the compound (A) is 20 mol % or more, it is possible to tightly form a bond with a functional group that may be present on the surface of a substrate, thereby more firmly bonding the substrates to each other.

[0087] When compound (A) contains secondary nitrogen atoms, the ratio of secondary nitrogen atoms in all nitrogen atoms in compound (A) is preferably 5 mol % to 50 mol %, more preferably 5 mol % to 30 mol %.

[0088] In addition to primary nitrogen atoms and secondary nitrogen atoms, compound (A) may also contain tertiary nitrogen atoms. When compound (A) contains tertiary nitrogen atoms, the proportion of tertiary nitrogen atoms in all nitrogen atoms in compound (A) is preferably from 20 mol% to 50 mol%, and more preferably from 25 mol% to 45 mol%.

[0089] The content of compound (A) in the composition is not particularly limited as long as the ratio of the primary nitrogen atoms and secondary nitrogen atoms contained in compound (A) to the total of the primary nitrogen atoms and secondary nitrogen atoms contained in compound (A) and the primary nitrogen atoms contained in compound (C) is 3 mol% to 95 mol%.

[0090] From the viewpoint of the balance between the thermal expansion coefficient and the bonding strength, the ratio is preferably 5 mol % to 75 mol %, more preferably 10 mol % to 50 mol %.

[0091] (Compound (B))

[0092] Compound (B) is a compound having 3 or more -C(=O)OX groups (X is a hydrogen atom or an alkyl group having 1 to 6 carbon atoms) in the molecule, and among the 3 or more -C(=O)OX groups (hereinafter also referred to as "COOX"), 1 to 6 are -C(=O)OH groups (hereinafter also referred to as "COOH").

[0093] When the compound (B) has a -C(=O)OX group (X is a hydrogen atom or an alkyl group having 1 to 6 carbon atoms) in the molecule, the solubility in the composition is improved.

[0094] The compound (B) may be used alone or in combination of two or more.

[0095] Compound (B) is a compound having 3 or more -C(=O)OX groups (X is a hydrogen atom or an alkyl group having 1 to 6 carbon atoms) in the molecule, preferably a compound having 3 or more -C(=O)OX groups in the molecule, and more preferably a compound having 3 or 4 -C(=O)OX groups in the molecule.

[0096] When the compound (B) has three or four -C(=O)OX groups in the molecule, it can react efficiently with the compound (A).

[0097] In compound (B), X in the -C(=O)OX group may be a hydrogen atom or an alkyl group having 1 to 6 carbon atoms, preferably a hydrogen atom, a methyl group, an ethyl group, or a propyl group. It should be noted that X in the -C(=O)OX group may be the same or different.

[0098] Compound (B) is a compound having 1 or more and 6 or less -C(=O)OH groups in which X is a hydrogen atom in the molecule, preferably a compound having 1 or more and 4 or less -C(=O)OH groups in the molecule, more preferably a compound having 2 or more and 4 or less -C(=O)OH groups in the molecule, and further preferably a compound having 2 or 3 -C(=O)OH groups in the molecule.

[0099] When the compound (B) has 1 to 4 -C(=O)OH groups in the molecule, the solubility in the composition will be improved.

[0100] The weight average molecular weight of compound (B) is not particularly limited. For example, the weight average molecular weight of compound (B) may be 200 to 600, 200 to 500, 200 to 450, or 200 to 400.

[0101] When the weight average molecular weight of the compound (B) is within the above range, the solubility in the composition will be improved.

[0102] The compound (B) preferably has a ring structure in the molecule. Examples of the ring structure include an alicyclic structure and an aromatic ring structure. In addition, the compound (B) may have multiple ring structures in the molecule, and the multiple ring structures may be the same or different.

[0103] When the compound (B) has a ring structure in the molecule, the heat resistance of the cured product will be improved.

[0104] As the alicyclic structure, for example, an alicyclic structure having 3 to 8 carbon atoms can be cited, preferably an alicyclic structure having 4 to 6 carbon atoms, and the ring structure may be saturated or unsaturated. More specifically, as the alicyclic structure, saturated alicyclic structures such as a cyclopropane ring, a cyclobutane ring, a cyclopentane ring, a cyclohexane ring, a cycloheptane ring, and a cyclooctane ring can be cited; and unsaturated alicyclic structures such as a cyclopropene ring, a cyclobutene ring, a cyclopentene ring, a cyclohexene ring, a cycloheptene ring, and a cyclooctene ring can be cited.

[0105] The aromatic ring structure is not particularly limited as long as it is a ring structure showing aromaticity, and examples thereof include benzene-based aromatic rings such as benzene ring, naphthalene ring, anthracene ring, and perylene ring, aromatic heterocyclic rings such as pyridine ring and thiophene ring, and non-benzene-based aromatic rings such as indene ring and azulene ring.

[0106] The ring structure possessed by the compound (B) in the molecule is preferably at least one selected from the group consisting of a cyclobutane ring, a cyclopentane ring, a cyclohexane ring, a benzene ring and a naphthalene ring. From the viewpoint of further improving the heat resistance of the cured product, at least one of a benzene ring and a naphthalene ring is more preferred.

[0107] As described above, the compound (B) may have a plurality of ring structures in the molecule, and when the ring structure is benzene, the compound (B) may have a biphenyl structure, a benzophenone structure, a diphenyl ether structure, or the like.

[0108] Compound (B) may have fluorine atoms in the molecule. For example, it may have 1 or more and 6 or less fluorine atoms in the molecule, or it may have 3 or more and 6 or less fluorine atoms in the molecule. For example, compound (B) may have a fluoroalkyl group in the molecule, specifically, a trifluoroalkyl group or a hexafluoroisopropyl group.

[0109] When the compound (B) has a fluorine atom in the molecule, the water absorption of the cured product decreases.

[0110] Furthermore, as compound (B), carboxylic acid compounds such as alicyclic carboxylic acids, benzene carboxylic acids, naphthalene carboxylic acids, diphthalic acids, and fluorinated aromatic ring carboxylic acids; carboxylate compounds such as alicyclic carboxylic acid esters, benzene carboxylic acid esters, naphthalene carboxylic acid esters, diphthalic acid esters, and fluorinated aromatic ring carboxylic acid esters. It should be noted that the carboxylate compound is a compound having a carboxyl group (-C(=O)OH group) in the molecule, and in more than 3 -C(=O)OX groups, at least one X is an alkyl group with a carbon number of 1 to 6 (i.e., having an ester bond). In the present embodiment, since compound (B) is a carboxylate compound, the agglomeration caused by the association of compound (A) and compound (B) is suppressed, the agglomerates and pits are reduced, and the film thickness is easily adjusted.

[0111] The carboxylic acid compound is preferably a 4-valent or less carboxylic acid compound containing 4 or less -C(=O)OH groups, and more preferably a 3- or 4-valent carboxylic acid compound containing 3 or 4 -C(=O)OH groups.

[0112] The carboxylic acid ester compound is preferably a compound containing 3 or less carboxyl groups (—C(═O)OH groups) and 3 or less ester bonds in the molecule, and more preferably a compound containing 2 or less carboxyl groups and 2 or less ester bonds in the molecule.

[0113] In addition, for the carboxylate compound, among the three or more -C(=O)OX groups, when X is an alkyl group having 1 to 6 carbon atoms, X is preferably a methyl group, an ethyl group, a propyl group, a butyl group, etc., and from the viewpoint of further suppressing the aggregation caused by the association of the compound (A) and the compound (B), an ethyl group or a propyl group is preferred.

[0114] Specific examples of the carboxylic acid compound include, but are not limited to, alicyclic carboxylic acids such as 1,2,3,4-cyclobutanetetracarboxylic acid, 1,2,3,4-cyclopentanetetracarboxylic acid, 1,3,5-cyclohexanetricarboxylic acid, 1,2,4-cyclohexanetricarboxylic acid, 1,2,4,5-cyclohexanetetracarboxylic acid, and 1,2,3,4,5,6-cyclohexanehexacarboxylic acid; phenylcarboxylic acids such as 1,2,4-benzenetricarboxylic acid, 1,3,5-benzenetricarboxylic acid, pyromellitic acid, benzenepentacarboxylic acid, and benzenehexacarboxylic acid; naphthylcarboxylic acids such as 1,4,5,8-naphthalenetetracarboxylic acid and 2,3,6,7-naphthalenetetracarboxylic acid; Acid; 3,3',5,5'-tetracarboxydiphenylmethane, biphenyl-3,3',5,5'-tetracarboxylic acid, biphenyl-3,4',5-tricarboxylic acid, biphenyl-3,3',4,4'-tetracarboxylic acid, benzophenone-3,3',4,4'-tetracarboxylic acid, 4,4'-oxydiphthalic acid, 3,4'-oxydiphthalic acid, 1,3-bis(phthalic acid)tetramethyldisiloxane, 4,4'-(ethynyl-1,2-diyl)diphthalic acid (4,4'-(Ethyne-1,2-diyl) diphthalic acid acid), 4,4'-(1,4-phenylenebis(oxy))diphthalic acid), 4,4'-([1,1'-biphenyl]-4,4'-diylbis(oxy))diphthalic acid), 4,4'-((oxybis(4,1-phenylene))bis(oxy))diphthalic acid acid); perylene carboxylic acids such as perylene-3,4,9,10-tetracarboxylic acid; anthracene carboxylic acids such as anthracene-2,3,6,7-tetracarboxylic acid; and fluorinated aromatic ring carboxylic acids such as 4,4'-(hexafluoroisopropylidene)diphthalic acid, 9,9-bis(trifluoromethyl)-9H-xanthene-2,3,6,7-tetracarboxylic acid and 1,4-bis(trifluoromethyl)pyromellitic acid.

[0115] Specific examples of the carboxylic acid ester compound include compounds in which at least one carboxyl group in the specific examples of the carboxylic acid compound is substituted with an ester group. Examples of the carboxylic acid ester compound include half-esterified compounds represented by the following general formulas (B-1) to (B-6).

[0116] [Chemistry 5]

[0117]

[0118] R in general formulae (B-1) to (B-6) are each independently an alkyl group having 1 to 6 carbon atoms, among which methyl, ethyl, propyl and butyl are preferred, and ethyl and propyl are more preferred.

[0119] The half-esterified compound can be produced by, for example, mixing carboxylic anhydride, which is an anhydride of the above-mentioned carboxylic acid compound, with an alcohol solvent and ring-opening the carboxylic anhydride.

[0120] The content of the compound (B) in the composition is preferably an amount such that the ratio (COOH / N) of the carboxyl equivalent number (COOH) of the compound (B) to the total amine equivalent number (N) of the compound (A) and the compound (C) is 0.1 to 3.0, more preferably 0.3 to 2.5, and even more preferably 0.4 to 2.2. When COOH / N is 0.1 to 3.0, a crosslinked structure based on the reaction of the compound (A), the compound (B) and the compound (C) is sufficiently formed, and a cured product having excellent heat resistance and insulation properties tends to be obtained.

[0121] (Compound (C))

[0122] The compound (C) is a compound having a ring structure and one or more primary nitrogen atoms directly bonded to the ring structure.

[0123] The compound (C) reacts with the compound (B) together with the compound (A) to form a cured product.

[0124] The compound (C) has a ring structure and one or more primary nitrogen atoms directly bonded to the ring structure. It is considered that the rigidity of the cured product increases and the thermal expansion coefficient decreases by introducing the structure into the cured product.

[0125] The compound (C) may be used alone or in combination of two or more.

[0126] In the present disclosure, the "primary nitrogen atom directly bonded to the ring structure" means a primary nitrogen atom (-NH2) bonded to the ring structure by a single bond (ie, not via a carbon atom or the like).

[0127] The number of primary nitrogen atoms directly bonded to the ring structure in the molecule of compound (C) is not particularly limited as long as it is 1 or more. From the viewpoint of increasing the crosslinking density, it is preferably 2 or more, and more preferably a diamine compound having 2 primary amino groups or a triamine compound having 3 primary amino groups.

[0128] Compound (C) may have one ring structure or multiple ring structures in the molecule. When compound (C) has multiple ring structures in the molecule, it may have a cationic functional group containing a primary nitrogen atom directly bonded to each ring structure, or may have a cationic functional group containing a primary nitrogen atom directly bonded to only one ring structure.

[0129] When compound (C) has multiple ring structures in the molecule, the multiple ring structures may be the same or different, or may form a condensed ring. Alternatively, the multiple ring structures may be linked by a single bond or via a linking group such as an ether group, a carbonyl group, a sulfonyl group, or a methylene group.

[0130] Examples of the ring structure contained in the compound (C) include an alicyclic structure, an aromatic ring (including a heterocyclic ring) structure, and condensed ring structures thereof.

[0131] Examples of the alicyclic structure include an alicyclic structure having 3 to 8 carbon atoms, preferably 4 to 6 carbon atoms. The ring structure may be saturated or unsaturated. More specifically, examples include saturated alicyclic structures such as a cyclopropane ring, a cyclobutane ring, a cyclopentane ring, a cyclohexane ring, a cycloheptane ring, and a cyclooctane ring; and unsaturated alicyclic structures such as a cyclopropene ring, a cyclobutene ring, a cyclopentene ring, a cyclohexene ring, a cycloheptene ring, and a cyclooctene ring.

[0132] Examples of the aromatic ring structure include an aromatic ring structure having a carbon number of 6 to 20, preferably an aromatic ring structure having a carbon number of 6 to 10. Specifically, examples include benzene-based aromatic ring structures such as a benzene ring, a naphthalene ring, an anthracene ring, and a perylene ring, and non-benzene-based aromatic ring structures such as a pyridine ring, a thiophene ring, an indene ring, and an azulene ring.

[0133] Examples of the heterocyclic structure include 3-membered to 10-membered, preferably 5-membered or 6-membered heterocyclic structures. Examples of heteroatoms contained in the heterocyclic ring include sulfur atoms, nitrogen atoms, and oxygen atoms, and these may be either one or two or more.

[0134] Specific examples of the heterocyclic structure include: azole ring, thiophene ring, pyrrole ring, pyrrolidine ring, pyrazole ring, imidazole ring, triazole ring, isocyanuric acid ring, pyridine ring, pyridazine ring, pyrimidine ring, pyrazine ring, piperidine ring, piperazine ring, triazine ring, indole ring, indoleline ring, quinoline ring, acridine ring, naphthyridine ring, quinazoline ring, purine ring, quinoxaline ring, etc.

[0135] As all the ring structures in the molecule of compound (C), benzene ring, cyclohexane ring and benzophenone ring are more preferred. Azole ring.

[0136] The ring structure in the molecule of the compound (C) may have a substituent other than the primary nitrogen atom, for example, an alkyl group having 1 to 6 carbon atoms, an alkyl group substituted with a halogen atom, or the like.

[0137] The weight average molecular weight of the compound (C) is not particularly limited and may be, for example, 80 to 600, 90 to 500, or 100 to 450.

[0138] Examples of the compound (C) include alicyclic amines, aromatic cyclic amines, heterocyclic amines having a nitrogen-containing heterocyclic ring, and amine compounds having both a heterocyclic ring and an aromatic ring.

[0139] Specific examples of the alicyclic amine include cyclohexylamine and dimethylaminocyclohexane.

[0140] Specific examples of the aromatic cyclic amine include diaminodiphenyl ether, xylenediamine (preferably p-xylenediamine), diaminobenzene, diaminotoluene, methylenedianiline, dimethyldiaminobiphenyl, bis(trifluoromethyl)diaminobiphenyl, diaminobenzophenone, diaminobenzanilide, bis(aminophenyl)fluorene, bis(aminophenoxy)benzene, bis(aminophenoxy)biphenyl, dicarboxydiaminodiphenylmethane, diaminoresorcinol, dihydroxybenzidine, diaminobenzidine, 1,3,5-triaminophenoxybenzene, 2,2'-dimethylbenzidine, and tris(4-aminophenyl)amine.

[0141] Specific examples of the heterocyclic amine having a nitrogen-containing heterocyclic ring include melamine, ammeline, melam, melem, and tris(4-aminophenyl)amine.

[0142] Specific examples of the amine compound having both a heterocyclic ring and an aromatic ring include N2,N4,N6-tris(4-aminophenyl)-1,3,5-triazine-2,4,6-triamine, 2-(4-aminophenyl)benzotriazine, Oxazol-5-amine, etc.

[0143] The content of compound (C) in the composition is not particularly limited as long as the ratio of the primary nitrogen atoms contained in compound (A) to the total of the primary nitrogen atoms and secondary nitrogen atoms contained in compound (A) and the primary nitrogen atoms contained in compound (C) is 3 mol% to 95 mol%.

[0144] From the viewpoint of the balance between the thermal expansion coefficient and the bonding strength, the ratio is preferably 5 mol % to 75 mol %, more preferably 10 mol % to 50 mol %, and further preferably 10 mol % to 30 mol %.

[0145] (Polar solvent)

[0146] The composition may contain a polar solvent. In the present disclosure, the term "polar solvent" refers to a solvent having a relative dielectric constant of 5 or more at room temperature (25° C.).

[0147] If the composition contains a polar solvent, the solubility of the components in the composition is improved.

[0148] The polar solvent may be used alone or in combination of two or more.

[0149] As the polar solvent, specifically, there can be mentioned protic solvents such as water and heavy water; alcohols such as methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, isobutanol, isopentanol, cyclohexanol, ethylene glycol, propylene glycol, 2-methoxyethanol, 2-ethoxyethanol, benzyl alcohol, diethylene glycol, triethylene glycol, and glycerol; ethers such as tetrahydrofuran and dimethoxyethane; aldehydes and ketones such as furfural, acetone, ethyl methyl ketone, and cyclohexanone; acid derivatives such as acetic anhydride, ethyl acetate, butyl acetate, ethylene carbonate, propylene carbonate, formaldehyde, N-methylformamide, N,N-dimethylformamide, N-methylacetamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, and hexamethylphosphoramide; nitriles such as acetonitrile and propionitrile; and nitro compounds such as nitromethane and nitrobenzene; sulfur compounds such as dimethyl sulfoxide.

[0150] As the polar solvent, a protic solvent is preferably contained, water is more preferably contained, and ultrapure water is further preferably contained.

[0151] When the composition contains a polar solvent, the content thereof is not particularly limited, and for example, may be 1.0% by mass to 99.99896% by mass, or 40% by mass to 99.99896% by mass, based on the entire composition.

[0152] (additive)

[0153] The composition may contain additives as necessary. Examples of the additives include acids having a carboxyl group and a weight average molecular weight of 46 to 195, and bases having a nitrogen atom and a weight average molecular weight of 17 to 120 and no ring structure.

[0154] It is speculated that the composition contains an acid having a weight average molecular weight of 46 to 195, so that the primary nitrogen atom or secondary nitrogen atom of compound (A) and compound (C) forms an ionic bond with the carboxyl group in the acid, thereby suppressing the aggregation caused by the association of compound (A) and compound (C) with compound (B). In more detail, it is speculated that the interaction (for example, electrostatic interaction) between the ammonium ions derived from compound (A) and compound (C) and the carboxylate ions derived from the carboxyl group in the acid is stronger than the interaction between the ammonium ions derived from compound (A) and compound (C) and the carboxylate ions derived from the carboxyl group in compound (B), so aggregation is suppressed. It should be noted that the present invention is not limited by the above speculation.

[0155] The type of acid having a weight average molecular weight of 46 or more and 195 or less having a carboxyl group is not particularly limited, and examples thereof include monocarboxylic acid compounds, dicarboxylic acid compounds, oxydicarboxylic acid compounds, etc. More specifically, examples thereof include formic acid, acetic acid, malonic acid, oxalic acid, benzoic acid, lactic acid, glycolic acid, glyceric acid, butyric acid, methoxyacetic acid, ethoxyacetic acid, phthalic acid, terephthalic acid, picolinic acid, salicylic acid, 3,4,5-trihydroxybenzoic acid, etc. (excluding compounds corresponding to compound (B)).

[0156] When the composition contains an acid having a weight average molecular weight of 46 to 195, its content is not particularly limited. For example, it is preferably an amount such that the ratio of the number of carboxyl groups of the acid to the total number of primary nitrogen atoms and secondary nitrogen atoms of compound (A) and compound (C) (COOH / N) is 0.01 to 10, more preferably 0.02 to 6, and even more preferably 0.5 to 3.

[0157] It is speculated that the composition contains a base having a weight average molecular weight of 17 to 120 and having a nitrogen atom, so that the carboxyl group of compound (B) forms an ionic bond with the amino group of the base, thereby suppressing the aggregation caused by the association of compound (A) and compound (C) with compound (B). In more detail, it is speculated that the interaction between the carboxyl ion derived from the carboxyl group in compound (B) and the ammonium ion derived from the amino group in the base is stronger than the interaction between the ammonium ion derived from compound (A) and compound (C) and the carboxyl ion derived from the carboxyl group in compound (B), so aggregation is suppressed. It should be noted that the present invention is not limited by the above speculation.

[0158] The type of the compound having a nitrogen atom and a weight average molecular weight of 17 to 120 is not particularly limited, and examples thereof include monoamine compounds, diamine compounds, and the like (excluding compounds corresponding to compound (A) and compound (C)). More specifically, examples thereof include ammonia, ethylamine, ethanolamine, diethylamine, triethylamine, ethylenediamine, N-acetylethylenediamine, N-(2-aminoethyl)ethanolamine, and N-(2-aminoethyl)glycine.

[0159] When the composition contains a base having a weight average molecular weight of 17 to 120, its content is not particularly limited. For example, the ratio of the number of nitrogen atoms in the base to the number of carboxyl groups in compound (B) (N / COOH) is preferably 0.5 to 5, more preferably 0.9 to 3.

[0160] (Other ingredients)

[0161] When selectivity of plasma etching resistance is required for the composition (for example, when used as a gap-filling material or a buried insulating film), a metal alkoxide represented by the following general formula (I) may be contained.

[0162] R1 n M(OR2) m-n ···(I) (wherein, R1 is a non-hydrolyzable group, R2 is an alkyl group having 1 to 6 carbon atoms, M represents at least one metal atom selected from the group consisting of Ti, Al, Zr, Sr, Ba, Zn, B, Ga, Y, Ge, Pb, P, Sb, V, Ta, W, La, Nd and In metal atoms, m is the valence of the metal atom M and is 3 or 4, when m is 4, n is an integer of 0 to 2, when m is 3, n is 0 or 1, when there are multiple R1s, each R1 may be the same as or different from each other, and when there are multiple OR2s, each OR2 may be the same as or different from each other.)

[0163] When the film produced from the composition requires insulation properties (for example, for use as a through silicon via insulating film or a buried insulating film), a silane compound (excluding compounds corresponding to compound (A)) may be contained to improve insulation properties or mechanical strength.

[0164] Specific examples of the silane compound include tetraethoxysilane, tetramethoxysilane, bis(triethoxysilyl)ethane, bis(triethoxysilyl)methane, bis(methyldiethoxysilyl)ethane, 1,1,3,3,5,5-hexaethoxy-1,3,5-trisilacyclohexane, 1,3,5,7-tetramethyl-1,3,5,7-tetrahydroxycyclosiloxane, 1,1,4,4-tetramethyl-1,4-diethoxydisiloxane, 1,3,5-trimethyl-1,3,5-trimethyl-1,3,5-triethoxy-1,3,5-trisilacyclohexane, and silane coupling agents having functional groups other than amino groups (epoxy groups, mercapto groups, etc.).

[0165] The composition may contain a solvent other than the polar solvent. Examples of the solvent other than the polar solvent include n-hexane and the like.

[0166] The composition may contain benzotriazole or a derivative thereof, for example, to inhibit copper corrosion.

[0167] The pH of the composition is not particularly limited, but is preferably 2.0 or more and 12.0 or less.

[0168] When the pH of the composition is 2.0 or more and 12.0 or less, damage to the substrate due to the composition can be suppressed.

[0169] In the composition, the content of sodium and potassium is preferably 10 ppb by mass or less based on each element. If the content of sodium and potassium is 10 ppb by mass or less based on each element, the occurrence of poor electrical characteristics of the semiconductor device such as malfunction of the transistor can be suppressed.

[0170] When the composition contains components other than compound (A), compound (B) and compound (C), the total mass of compound (A), compound (B) and compound (C) is preferably 50% by mass or more of the total mass of non-volatile components in the composition, more preferably 70% by mass or more, more preferably 80% by mass or more. In the present disclosure, the so-called "non-volatile component" refers to components other than components (solvents, etc.) that are removed when the composition becomes a cured product.

[0171] (Use of the composition)

[0172] The use of the composition of this embodiment is not particularly limited, and can be used for various uses including the manufacture of semiconductor devices. For example, it can be used to form a layer on a substrate or between substrates, and can also be used to manufacture a laminated body described later.

[0173] <Laminated body>

[0174] The laminate of the present embodiment is a laminate comprising a layer (hereinafter also referred to as a cured product layer) and a substrate, wherein the layer comprises a reaction product of a compound (A), a compound (B) and a compound (C), wherein the compound (A) has a cationic functional group comprising at least one selected from a primary nitrogen atom and a secondary nitrogen atom and an Si-O bond, the compound (B) has three or more -C(=O)OX groups (X is a hydrogen atom or an alkyl group having 1 to 6 carbon atoms), of which one or more of the three or more -C(=O)OX groups are -C(=O)OH groups, and the compound (C) has a ring structure and one or more primary nitrogen atoms directly bonded to the ring structure, and the ratio of the primary nitrogen atoms and secondary nitrogen atoms contained in the compound (A) to the total of the primary nitrogen atoms and secondary nitrogen atoms contained in the compound (A) before the reaction and the primary nitrogen atoms contained in the compound (C) is 3 mol% to 95 mol%.

[0175] The details and preferred embodiments of each compound as a starting material of the reaction product are the same as those of each compound contained in the above-mentioned composition. The layer containing the reaction product may contain the components that may be contained in the above-mentioned composition as necessary.

[0176] The cured product layer is configured to be bonded to the substrate in a manner of contacting the surface of the substrate. As described above, the cured product layer obtained by the composition of the present embodiment has a low coefficient of thermal expansion, so it is not easy to generate strain caused by the difference in coefficient of thermal expansion with the substrate on the bonding surface, and the reliability of the laminate is excellent.

[0177] The number of substrates included in the laminate is not particularly limited, and may be 1 or plural. When there are 2 or more substrates, the materials thereof may be the same or different.

[0178] From the viewpoint of fully achieving the effects of the present invention, the substrate preferably has a thermal expansion coefficient that is equal to or smaller than that of the cured material layer.

[0179] In one embodiment of the laminated body, the substrate includes a first substrate and a second substrate, and the first substrate, the cured material layer (layer including a reaction product), and the second substrate are arranged in this order.

[0180] Examples of the material of the substrate include inorganic materials, organic materials, and composites thereof.

[0181] Specifically, inorganic materials include: semiconductors such as Si, InP, GaN, GaAs, InGaAs, InGaAlAs, SiGe, and SiC; oxides, carbides, or nitrides such as borosilicate glass (Pyrex (registered trademark)), quartz glass (SiO2), sapphire (Al2O3), ZrO2, Si3N4, AlN, and MgAl2O4; piezoelectrics or dielectrics such as BaTiO3, LiNbO3, SrTiO3, and LiTaO3; diamond; metals such as Al, Ti, Fe, Cu, Ag, Au, Pt, Pd, Ta, and Nb; carbon, etc.

[0182] Specific examples of the organic material include polydimethylsiloxane (PDMS), epoxy resin, phenolic resin, polyimide, benzocyclobutene resin, polybenzoic acid, Azoles, etc.

[0183] The main uses of each material are as follows.

[0184] Si is used in semiconductor memory, LSI stacking, CMOS image sensors, MEMS sealing, optical devices, LEDs, etc.;

[0185] SiO2 is used in semiconductor memory, LSI stacking, MEMS sealing, microchannels, CMOS image sensors, optical devices, LEDs, etc.

[0186] BaTiO3, LiNbO3, SrTiO3, and LiTaO3 are used in surface elastic wave devices;

[0187] PDMS is used for microchannels;

[0188] InGaAlAs, InGaAs, and InP are used in optical devices;

[0189] InGaAlAs, GaAs, and GaN are used in LEDs, etc.

[0190] The surface of the substrate (at least the surface in contact with the cured product layer) preferably has at least one selected from the group consisting of a hydroxyl group, an epoxy group, a carboxyl group, an amino group, and a mercapto group. This can make the bonding strength with the cured product layer of the composition stronger.

[0191] The surface having hydroxyl groups can be obtained by subjecting the surface of the substrate to surface treatment such as plasma treatment, chemical treatment, and ozone treatment.

[0192] The surface having an epoxy group, a carboxyl group, an amino group, or a mercapto group can be obtained by surface-treating the surface of a substrate using a silane coupling agent or the like having an epoxy group, a carboxyl group, an amino group, or a mercapto group.

[0193] At least one selected from the group consisting of hydroxyl, epoxy, carboxyl, amino and mercapto groups is preferably in a state of being bonded to an element contained in the substrate, more preferably in a state of being bonded to at least one element selected from the group consisting of Si, Al, Ti, Zr, Hf, Fe, Ni, Cu, Ag, Au, Ga, Ge, Sn, Pd, As, Pt, Mg, In, Ta and Nb, and further preferably in a state of being a silanol group (Si-OH group) containing a hydroxyl group.

[0194] The substrate may have an electrode on at least one surface (preferably the side facing the cured product layer).

[0195] The thickness of the substrate is preferably 1 μm to 1 mm, more preferably 2 μm to 900 μm. In the case of a plurality of substrates, the above thickness is the thickness of each substrate, which may be the same or different.

[0196] The shape of the substrate is not particularly limited. For example, when the substrate is a silicon substrate, it can be a silicon substrate formed with an interlayer insulating layer (Low-k film). The substrate can be formed with fine grooves (recesses), fine through holes, etc.

[0197] The laminated body of the present embodiment may further include a substrate that is not in contact with the cured material layer. Preferred materials and other aspects of the substrate that is not in contact with the cured material layer are the same as those of the above-mentioned substrate.

[0198] The thickness of the cured product layer is not particularly limited and can be set according to the application, for example, it can be 0.1 nm to 20,000 nm, 0.5 nm to 10,000 nm, 5 nm to 5,000 nm, or 5 nm to 3,000 nm.

[0199] The content of the inorganic or resin filler having a maximum diameter of 0.3 μm or more in the cured layer is preferably 30% by mass or less, more preferably 10% by mass or less, and even more preferably 0% by mass of the entire cured layer.

[0200] If the content of the filler contained in the cured material layer is within the above range, even when the thickness of the cured material layer is reduced, poor bonding of the laminate can be suppressed. In addition, when the first substrate and the second substrate are laminated with the cured material layer, sometimes an instrument is used to identify the alignment marks formed on each substrate for positioning. At this time, if the content of the filler is within the above range, the transparency of the cured material layer is improved, and more accurate positioning can be performed.

[0201] The glass transition temperature (Tg) of the cured product layer is preferably 100°C to 400°C. If Tg is in the above temperature range, the elastic modulus of the film decreases when it undergoes a high temperature process, thereby reducing warping and internal stress of the laminate, and suppressing a decrease in bonding strength caused by peeling, etc. Tg is more preferably 100°C to 350°C, more preferably 120°C to 300°C, and more preferably 120°C to 250°C.

[0202] The Tg of the cured product layer is measured by the following method.

[0203] The composition was coated on a resin film and cured by baking at 350°C for 1 hour in a nitrogen atmosphere. Then, it was peeled off from the resin film to form a cured layer with a film thickness of 10 μm to 70 μm. A differential scanning calorimeter (DSC, DSC2500 manufactured by TA Instruments) was used to determine the heat flow (heating rate and cooling rate: 10°C / min) at 23°C to 400°C in a nitrogen atmosphere, and the Tg of the cured layer was determined from the temperature of the inflection point.

[0204] The water absorption of the cured product layer is preferably 3% by mass or less. If the water absorption is within the above numerical range, outgassing from the resin can be effectively suppressed, and the occurrence of defects such as voids and peeling of the laminate can be effectively suppressed. The water absorption is more preferably 2% by mass or less.

[0205] The water absorption of the cured layer was measured based on the water absorption standard test method (ASTM D570) from the mass change before and after immersing the cured layer obtained in the same manner as the Tg measurement in pure water (23° C., 24 hours).

[0206] The elastic modulus of the cured material layer at 250°C is preferably 0.01 GPa to 20 GPa. If the elastic modulus at 250°C is within the above numerical range, the internal stress during heating of the laminate can be reduced, and warping, peeling, failure of the device layer, etc. can be suppressed. The elastic modulus of the cured material layer at 250°C is more preferably 0.01 GPa to 12 GPa, and further preferably 0.1 GPa to 8 GPa.

[0207] The elastic modulus of the cured layer at 250° C. was measured by the following method using an atomic force microscope (AFM).

[0208] For the cured layer formed on the Si substrate, an AFM (trade name E-sweep, manufactured by SII Nanotech, AFM force curve surface scanning mode (force mapping mode), Si probe (equivalent to spring constant 2N / m)) was used to fit the force curve measurement results at a stage temperature of 250°C under vacuum using the DMT theoretical formula to calculate the elastic modulus.

[0209] The DMT theoretical formula is shown below. In the formula, E represents the elastic modulus of the resin film, ν represents the Poisson's ratio of the resin film, R represents the tip diameter of the cantilever, δ represents the indentation depth, F represents the force applied to the sample, and F c represents the maximum adhesion. Poisson's ratio is assumed to be 0.33.

[0210] [Number 1]

[0211]

[0212] The hardness of the cured layer at room temperature (23°C) is preferably 0.05 GPa to 1.8 GPa. If the hardness is within the above numerical range, the film can be prevented from breaking when an external force such as wire bonding is applied to the laminate. The hardness is more preferably 0.2 GPa to 1.5 GPa, and even more preferably 0.3 GPa to 1.0 GPa.

[0213] The hardness of the cured product layer is the hardness measured by the method (nanoindentation) in accordance with ISO14577.

[0214] Specifically, in a state where the cured layer is formed on a silicon substrate, a nanoindenter (Berkovich type indenter) is used to measure the unloading-displacement curve at 23°C under the condition of an indentation depth of 20nm. The hardness at 23°C is calculated from the maximum load according to the calculation method of the reference (Handbook of Micro / nano Tribology (Second Edition), edited by Bharat Bhushan, CRC Press). Hardness (H) is defined by the following formula. In the formula, P max Indicates the maximum load when the indentation depth is 20nm, A c It indicates the projected area of ​​the indenter on the specimen when pressed.

[0215] [Number 2]

[0216]

[0217] The elastic modulus of the cured layer at room temperature (23°C) is preferably 0.1 GPa to 20 GPa. If the elastic modulus of the cured layer at room temperature is within the above range, warping, peeling, etc. when external forces such as compression and shearing are applied to the laminate can be suppressed. The elastic modulus at room temperature is more preferably 0.5 GPa to 15 GPa, and further preferably 1 GPa to 10 GPa.

[0218] The elastic modulus of the cured layer at room temperature is obtained by measuring the unloading-displacement curve at 23° C. using a nanoindenter (Berkovich-type indenter) under the condition of a 20 nm indentation depth, while the cured layer is formed on a silicon substrate. The elastic modulus at 23° C. is calculated from the maximum load and the maximum displacement according to the calculation method of the reference (Handbook of Micro / nano Tribology (Second Edition), edited by Bharat Bhushan, CRC Press).

[0219] The elastic modulus is defined by the following formula. r Represents the elastic modulus, E i The Young's modulus of the indenter is 1140 GPa, ν i The Poisson's ratio of the pressure head is 0.07, E s and ν s represent the Young's modulus and Poisson's ratio of the specimen, respectively.

[0220] [Number 3]

[0221]

[0222] (Example of laminated structure)

[0223] The laminated body can be used for various purposes including components of semiconductor devices.

[0224] Examples of the laminated structure of substrate laminates in various applications are shown below.

[0225] For MEMS packaging: Si / cured layer / Si, SiO2 / cured layer / Si, SiO2 / cured layer / SiO2, Cu / cured layer / Cu,

[0226] For microchannel: PDMS / cured material layer / PDMS, PDMS / cured material layer / SiO2,

[0227] For CMOS image sensors: SiO2 / cured layer / SiO2, Si / cured layer / Si, SiO2 / cured layer / Si,

[0228] For through silicon via (TSV): SiO2 (with Cu electrode) / cured layer / SiO2 (with Cu electrode),

[0229] For memory and LSI: SiO2 / cured layer / SiO2,

[0230] For optical devices: (InGaAlAs, InGaAs, InP, GaAs) / cured layer / Si,

[0231] For LED: (InGaAlAs, GaAs, GaN) / cured layer / Si, (InGaAlAs, GaAs, GaN) / cured layer / SiO2, (InGaAlAs, GaAs, GaN) / cured layer / (Au, Ag, Al), (InGaAlAs, GaAs, GaN) / cured layer / sapphire,

[0232] For surface elastic wave devices: (BaTiO3, LiNbO3, SrTiO3, LiTaO3) / cured layer / (MgAl2O4, SiO2, Si, Al2O3).

[0233] In addition to the above-mentioned configuration, the laminate may further include a cured product formed as an insulating film on the surface of the substrate, in a recessed portion formed on the surface, in a through hole, and the like.

[0234] The cured product layer may be temporarily formed, for example, it may be used for applications such as a sacrificial film that is temporarily formed on a substrate during a semiconductor device manufacturing process and removed in a later process.

[0235] From the perspective of suppressing accidental peeling and reliability, the higher the tensile bonding strength of the laminate, the better. Specifically, the tensile bonding strength of the laminate is preferably 5 MPa or more, more preferably 10 MPa or more. The tensile bonding strength of the laminate can be obtained by measuring the yield point using a tensile testing machine. It should be noted that the tensile bonding strength can be 200 MPa or less, or 100 MPa or less.

[0236] From the viewpoint of suppressing the decrease in bonding strength due to outgassing, the outgassing pressure of the laminate is 2×10 - 6 The temperature of Pa is preferably 400°C or higher, more preferably 420°C or higher, and still more preferably 440°C or higher. The outgassing pressure is 2×10 -6 The temperature of Pa is the value measured under reduced pressure. -7 Pa. It should be noted that the pressure of the outgassing is 2×10 -6 The temperature of Pa may be 600° C. or lower, and may be 550° C. or lower.

[0237] The ratio of the total area of ​​the pores in the laminate (pore area ratio) is preferably 30% or less, more preferably 20% or less, and further preferably 10% or less. The pore area ratio is a value calculated by dividing the total area of ​​the pores by the total area of ​​the observed transmitted light in infrared light transmission observation and multiplying by 100. In the case where infrared light transmission observation is difficult, the reflected wave of an ultrasonic microscope, the transmitted wave of an ultrasonic microscope, or the reflected light of infrared light can be used, preferably the reflected wave of an ultrasonic microscope, and the pore area ratio can be calculated by the same method.

[0238] From the viewpoint of preventing accidental peeling and reliability, the higher the bonding strength of the laminate, the better. Specifically, when the bonding strength is expressed by surface energy, it is preferably 0.2 J / m 2 More preferably 0.5 J / m 2 More preferably, 1.0 J / m 2 Above, particularly preferably 2.5 J / m 2 above.

[0239] When the laminate includes the first substrate and the second substrate, the surface energy indicating the bonding strength between the first substrate and the second substrate is preferably within the above range. The surface energy of the laminate can be obtained by a blade insertion test described below.

[0240] <Method for producing laminate>

[0241] The method for producing a laminated body according to the present embodiment comprises: a first step of forming a layer z on a substrate or between substrates; and a second step of curing the layer, wherein the layer comprises a compound (A), a compound (B) and a compound (C).

[0242] The compound (A) has a cationic functional group including at least one selected from a primary nitrogen atom and a secondary nitrogen atom and a Si-O bond, the compound (B) has three or more -C(=O)OX groups (X is a hydrogen atom or an alkyl group having 1 to 6 carbon atoms), of which one or more and six are -C(=O)OH groups, and the compound (C) has a ring structure and one or more primary nitrogen atoms directly bonded to the ring structure, and the ratio of the primary nitrogen atoms and secondary nitrogen atoms contained in the compound (A) to the total of the primary nitrogen atoms and secondary nitrogen atoms contained in the compound (A) and the primary nitrogen atoms contained in the compound (C) is 3 mol% to 95 mol%.

[0243] The details and preferred embodiments of the substrate and compound used in the above method are the same as those described for the above composition and laminated body.

[0244] (First process)

[0245] The method for implementing the first process is not particularly limited. For example, compound (A), compound (B) and compound (C) can be applied together (i.e., in the state of the above-mentioned composition) on or between substrates to form a layer, or compound (A), compound (B) and compound (C) can be applied in multiple steps and formed on or between substrates. In the case where compound (A), compound (B) and compound (C) are applied in multiple steps, their order is not particularly limited. In addition, each can be applied separately, or any two components can be applied together. In the case where compound (A), compound (B) and compound (C) are applied in multiple steps, drying, cleaning, etc. can be implemented as needed after each step.

[0246] From the viewpoint of forming a layer of uniform thickness on or between substrates, the compound (A), the compound (B) and the compound (C) are preferably in the state of a solution. The solution can be prepared using, for example, a solvent that can be contained in the above composition.

[0247] The method for forming a layer comprising compound (A), compound (B) and compound (C) is not particularly limited and can be carried out by a commonly used method. For example, an immersion method, a spray method, a spin coating method, a rod coating method, etc. can be mentioned. Among them, in the case of forming a layer with a thickness of micrometer size, a rod coating method is preferably used, and in the case of forming a layer with a thickness of nanometer size (several nm to hundreds of nm), a spin coating method is preferably used.

[0248] The method of forming a layer by spin coating is not particularly limited. For example, the following method can be used: while the substrate is rotated by a spin coater, a solution is dripped onto the surface thereof, and then the substrate rotation speed is increased to dry the substrate. The conditions such as the rotation speed of the substrate, the amount of solution dripped and the dripping time, and the rotation speed of the substrate during drying are not particularly limited, and can be appropriately adjusted in consideration of the thickness of the layer to be formed.

[0249] (Second process)

[0250] In the second step, the layer containing compound (A), compound (B) and compound (C) is cured. Specifically, compound (A), compound (B) and compound (C) contained in the layer are reacted to form a layer containing their reaction products (cured material layer).

[0251] As a method for reacting the compound (A), the compound (B) and the compound (C), there is mentioned a method of heating at a temperature at which these components react (for example, 70° C. to 450° C.).

[0252] The temperature is preferably 100° C. to 450° C., more preferably 100° C. to 400° C., and even more preferably 150° C. to 350° C. Alternatively, the temperature may be 70° C. to 280° C., 80° C. to 250° C., or 90° C. to 2000° C.

[0253] The pressure during heating is not particularly limited. For example, it can be implemented at a pressure greater than the absolute pressure (17 Pa) and below atmospheric pressure. The pressure is preferably 1000 Pa or more and below atmospheric pressure, more preferably 5000 Pa or more and below atmospheric pressure, and further preferably 10000 Pa or more and below atmospheric pressure.

[0254] The heating method is not particularly limited and can be carried out by a common method using a furnace or a hot plate. As the furnace, for example, SPX-1120 manufactured by Apex Corporation, VF-1000LP manufactured by Koyo Heat Treatment Systems Co., Ltd., etc. can be used.

[0255] The heating in the heating step may be performed in an air atmosphere or in an inert gas (nitrogen, argon, helium, etc.) atmosphere.

[0256] The heating time is not particularly limited, and may be, for example, 3 hours or less, or 1 hour or less. The lower limit of the heating time is not particularly limited, and may be, for example, 30 seconds or more, or 3 minutes or more, or 5 minutes or more.

[0257] When heating at 70°C to 250°C, the heating time may be 300 seconds or less, 200 seconds or less, 120 seconds or less, or 80 seconds or less. In this case, the heating time may be 10 seconds or more, 20 seconds or more, or 30 seconds or more.

[0258] The heating temperature may be constant or variable. For example, a heating step at a low temperature (70° C. to 250° C.) and a heating step at a higher temperature (100° C. to 450° C.) may be provided.

[0259] In order to shorten the heating process, the compound (A), compound (B) and compound (C) applied on the substrate may be irradiated with ultraviolet light. As ultraviolet light, ultraviolet light with a wavelength of 170 nm to 230 nm, excimer light with a wavelength of 222 nm, excimer light with a wavelength of 172 nm, etc. are preferred. In addition, ultraviolet light irradiation is preferably performed under an inert gas atmosphere.

[0260] (Pressure process)

[0261] In the method for producing a laminate, the laminate is preferably pressed simultaneously with or after the second step (heating). Pressing the laminate increases the contact area between the substrate and the cured layer, thereby tending to further improve the bonding strength.

[0262] The pressing pressure when the laminate is pressed while being heated is preferably 0.1 MPa to 50 MPa, more preferably 0.1 MPa to 10 MPa, and even more preferably 0.1 MPa to 5 MPa. As a pressing device, for example, TEST MINI PRESS manufactured by Toyo Seiki Seisaku-sho Co., Ltd. can be used.

[0263] The heating temperature when the laminate is pressed while being heated is preferably 100° C. to 450° C., more preferably 100° C. to 400° C., and even more preferably 150° C. to 350° C. This tends to suppress damage to the semiconductor circuit when a semiconductor circuit is formed on the substrate.

[0264] The pressing pressure when the laminate is heated and pressed is preferably 0.1 MPa to 50 MPa, more preferably 0.1 MPa to 10 MPa. As a pressing device, for example, TEST MINI PRESS manufactured by Toyo Seiki Seisakusho can be used. In addition, there is no particular limitation on the pressing time, and for example, it can be set to 0.5 seconds to 1 hour.

[0265] The temperature when the laminate is pressed after heating is preferably 10° C. or higher and lower than 100° C., more preferably 10° C. to 70° C., further preferably 15° C. to 50° C., and particularly preferably 20° C. to 30° C. The above temperature refers to the temperature of the surface of the substrate to which the compound (A), the compound (B) and the compound (C) are attached.

[0266] (Post-heating process)

[0267] The method for producing a laminate may include a post-heating step of further heating the laminate after the second step. The provision of the post-heating step tends to provide a more excellent bonding strength.

[0268] The heating temperature in the post-heating step is preferably 100°C to 450°C, more preferably 150°C to 420°C, and even more preferably 150°C to 400°C.

[0269] The pressure during the post-heating step may be greater than the absolute pressure of 17 Pa and below atmospheric pressure, preferably 1000 Pa to below atmospheric pressure, more preferably 5000 Pa to below atmospheric pressure, and further preferably 10000 Pa to below atmospheric pressure.

[0270] In the post-heating step, it is preferred not to press the laminated body.

[0271] Example

[0272] Hereinafter, the present invention will be described in more detail with reference to Examples, but the present invention is not limited to these Examples.

[0273] (Preparation of Composition)

[0274] Compositions of Examples and Comparative Examples containing the components shown in Table 1 were prepared. The amounts of the components were adjusted so that the total amine equivalent of compound (A) and compound (C) was equal to the carboxyl equivalent of compound (B), and the ratio of the primary nitrogen atoms and secondary nitrogen atoms contained in compound (A) to the total of the primary nitrogen atoms and secondary nitrogen atoms contained in compound (A) and the primary nitrogen atoms contained in compound (C) was the value (mol %) shown in Table 1. The value (mass %) described for compound (A) is set to the value relative to compound (A).

[0275] Each composition contains water, ethanol and N,N-dimethylacetamide as polar solvents.

[0276] [Table 1]

[0277]

[0278] The details of the components shown in Table 1 are as follows.

[0279] 3APDES…3-Aminopropyldiethoxymethylsilane

[0280] 3APTES…3-Aminopropyltriethoxysilane

[0281] M3TMSPA…N-Methyl-3-(trimethoxysilyl)propylamine

[0282] ODPA…a half ester compound obtained by ring-opening 4,4'-oxydiphthalic anhydride with ethanol

[0283] BPDA…a half ester compound obtained by ring-opening 3,3',4,4'-biphenyltetracarboxylic dianhydride with ethanol

[0284] PMDA…a half ester compound obtained by ring-opening pyromellitic dianhydride with ethanol

[0285] TFDB…4,4'-Diamino-2,2'-bis(trifluoromethyl)biphenyl

[0286] AAPD…4,4'-Diamino-2,2'-dimethylbiphenyl

[0287] pXDA…p-Xylenediamine

[0288] (Evaluation of bonding strength)

[0289] The composition is applied on a silicon substrate (substrate 1) by spin coating, and another silicon substrate (substrate 2) is arranged thereon, and heated to 250°C while being pressurized at 1 MPa to obtain a laminate having a cured layer arranged between substrates 1 and 2. Next, according to the method described in the existing report (Journal of Applied Physics, 64 (1988) 4943-4950), the surface energy of the bonding interface between the substrate and the cured layer is measured by a blade insertion test as an indicator of bonding strength. Specifically, a blade with a thickness of 0.25 mm is inserted between substrate 1 and substrate 2, and an infrared light source and an infrared camera are used to measure the distance at which substrate 1 and substrate 2 peel off from the tip of the blade, and the surface energy is measured based on the following formula. The larger the value of the surface energy, the greater the bonding strength to the substrate. If it is 0.2 J / m 2 The above results indicate that the bonding strength is sufficient.

[0290] γ=3×10 9 ×t b 2 ×E 2 ×t 6 / (32×L 4 ×E×t 3 )

[0291] Here, γ represents the surface energy (J / m 2 ), t b represents the thickness of the blade (m), E represents the Young's modulus of substrate 1 and substrate 2 (GPa), t represents the total thickness of substrate 1 and substrate 2 (m), and L represents the distance from the blade tip where substrate 1 and substrate 2 peel off (m).

[0292] (Evaluation of thermal expansion coefficient)

[0293] The composition was applied to one side of a polyimide film (Ube Industries, Ltd., "Upilex") by spin coating and heated at 350°C to form a cured layer having a thickness of 13 μm to 40 μm. Next, the cured layer was peeled off from the polyimide film to obtain a self-supporting film. The average linear expansion coefficient (CTE) at 250°C was measured in a nitrogen atmosphere using a thermomechanical analysis (TMA) device (manufactured by Hitachi High-Tech Sciences, TMA7100C). The smaller the value of CTE, the smaller the thermal expansion coefficient. The results are shown in Table 1.

[0294] As shown in Table 1, the examples using the composition equivalent to the composition of the present embodiment have a smaller CTE of the cured layer than Comparative Example 1 using a composition not containing compound (C) and Comparative Example 2 using a composition containing a diamine compound not directly bonded to a ring structure instead of compound (C), and can be evaluated as having a lower thermal expansion coefficient.

[0295] Furthermore, the examples using the composition corresponding to the composition of the present embodiment have larger surface energy than Comparative Example 3 using a composition not containing the compound (A), and can be evaluated as having more excellent bonding strength.

[0296] The entire contents disclosed in Japanese Patent Application No. 2020-152329 are incorporated into this specification by reference.

[0297] All documents, patent applications, and technical standards described in this specification are incorporated into this specification by reference to the same extent as if each document, patent application, and technical standard was specifically and individually described as being incorporated by reference.

Claims

1. A composition comprising compound (A), compound (B) and compound (C), The compound (A) has a cationic functional group including at least one selected from a primary nitrogen atom and a secondary nitrogen atom and a Si—O bond, The compound (B) has three or more -C(=O)OX groups, wherein X is a hydrogen atom or an alkyl group having 1 to 6 carbon atoms, and among the 3 or more -C(=O)OX groups, 1 to 6 are -C(=O)OH groups. The compound (C) has a ring structure and one or more primary nitrogen atoms directly bonded to the ring structure, The ratio of the primary nitrogen atoms and secondary nitrogen atoms contained in the compound (A) to the total of the primary nitrogen atoms and secondary nitrogen atoms contained in the compound (A) and the primary nitrogen atoms contained in the compound (C) is 10 mol % to 95 mol %. 2 . The composition according to claim 1 , wherein compound (C) has two or more primary nitrogen atoms directly bonded to the ring structure. 3 . The composition according to claim 1 , wherein the weight average molecular weight of the compound (C) is 80 or more and 600 or less. 4 . The composition according to claim 1 , wherein the compound (A) has two alkyl groups bonded to the oxygen atom constituting the Si—O bond. 5 . The composition according to claim 1 , wherein the weight average molecular weight of the compound (B) is 200 to 600. The composition according to claim 1 or 2, further comprising a polar solvent.

7. The composition according to claim 1 or 2, which is used for manufacturing a semiconductor device.

8. The composition according to claim 1 or 2, which is used to form a layer on or between substrates.

9. A laminate comprising a layer and a substrate, The layer comprises a reaction product of compound (A), compound (B) and compound (C), The compound (A) has a cationic functional group including at least one selected from a primary nitrogen atom and a secondary nitrogen atom and a Si—O bond, The compound (B) has three or more -C(=O)OX groups, wherein X is a hydrogen atom or an alkyl group having 1 to 6 carbon atoms, and among the 3 or more -C(=O)OX groups, 1 to 6 are -C(=O)OH groups. The compound (C) has a ring structure and one or more primary nitrogen atoms directly bonded to the ring structure, The ratio of the primary nitrogen atoms and secondary nitrogen atoms contained in the compound (A) to the total of the primary nitrogen atoms and secondary nitrogen atoms contained in the compound (A) before the reaction and the primary nitrogen atoms contained in the compound (C) is 10 mol% to 95 mol%. 10 . The laminated body according to claim 9 , wherein the substrate includes a first substrate and a second substrate, and the first substrate, the layer including the reaction product, and the second substrate are arranged in this order.

11. A method for producing a laminate, comprising: a step of forming a layer on a substrate or between substrates; and a step of curing the layer. The layer comprises compound (A), compound (B) and compound (C), The compound (A) has a cationic functional group including at least one selected from a primary nitrogen atom and a secondary nitrogen atom and a Si—O bond, The compound (B) has three or more -C(=O)OX groups, wherein X is a hydrogen atom or an alkyl group having 1 to 6 carbon atoms, and among the 3 or more -C(=O)OX groups, 1 or more and 6 or less are -C(=O)OH groups, The compound (C) has a ring structure and one or more primary nitrogen atoms directly bonded to the ring structure, The ratio of the primary nitrogen atoms and secondary nitrogen atoms contained in the compound (A) to the total of the primary nitrogen atoms and secondary nitrogen atoms contained in the compound (A) and the primary nitrogen atoms contained in the compound (C) is 10 mol % to 95 mol %.

Citation Information

Patent Citations

  • Semiconductor device and manufacturing method therefor

    JP2010226060A

  • Adhesive composition for semiconductor

    JP2016047895A

  • Movable body

    JP2020152329A

  • Photosensitive resin composition

    JP1994308731A

  • Production of imide (Amide) resin, and energy-ray-curable resin composition prepared therefrom

    JP2000344889A