An ion intercalation exfoliation of MoS 2 Method for obtaining sheet-like structure
By using Zn2+ and Cs+ as interlayers in hydrothermal reactions, combining sodium carboxymethylcellulose, weakening the interlayer force of MoS2 at high temperature and using ultrasonic peeling, the low preparation efficiency and yield of MoS2 sheet structures in the prior art are solved. The problem of insufficient results has achieved efficient and fast preparation of MoS2 sheet structure, improving product quality and feasibility of large-scale production.
Patent Information
- Application Number
- CN202310106381.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-13
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-02-13
AI Technical Summary
In the preparation of single-layer MoS2, the mechanical peeling yield is low and the structure is easy to damage, the ion interpolation operation is complex and not easy to scale, the product quality of liquid ultrasonic method is poor, the equipment for chemical vapor deposition is demanding and high cost, which is difficult to Achieve efficient and fast preparation of MoS2 sheet structure.
Zn2+ and Cs+ are used as intercalation agents, combined with sodium carboxymethylcellulose, and the van der Waals force between the MoS2 layers is weakened at high temperature through hydrothermal reaction. Ultrasonic peeling is used to obtain a sheet-like structure, and then vacuum filtration is carried out to remove excess intercalation agent. Protect the crystal structure.
It improves the peeling efficiency and product quality of MoS2, maintains the integrity of the crystal structure, is suitable for large-scale production, and enhances the catalytic, cell and optical application performance of MoS2.
Smart Images

Figure CN115959708B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nano material preparation, and relates to a method for preparing a flaky structure, in particular to a method for obtaining a flaky structure by ion intercalation exfoliation of MoS2. Background Art
[0002] Molybdenum disulfide (MoS2) is a semiconductor nanomaterial with a layered structure. The layers are bound by weak van der Waals forces. Each layer of MoS2 molecules consists of three atomic layers. The "sandwich" structure of two layers of sulfur atoms sandwiching a layer of molybdenum atoms, with 6 sulfur atoms distributed around each molybdenum atom and 3 molybdenum atoms distributed around each sulfur atom, is bound by strong covalent bonds. The thickness of each layer of MoS2 is about 0.65nm. MoS2 has three crystal structures: 1T-type MoS2, 2H-type MoS2 and 3R-type MoS2, of which 2H-type MoS2 is a stable state with semiconductor properties. In 2H-type MoS2, Mo atoms are triangular prisms with six coordinations, and 2 S-Mo-S units constitute a unit cell. The band gap of MoS2 is 1.2-1.92eV, the bandgap width is 1.29eV, and it has good mechanical properties and high electron mobility. Therefore, MoS2 nanosheets are widely used in field effect transistors, sensors, battery electrodes, optics and other fields due to their excellent lubrication and catalytic properties.
[0003] So far, the methods for preparing single-layer MoS2 exfoliation are mechanical exfoliation, ion intercalation, liquid phase exfoliation and chemical vapor deposition. Among them, the physical exfoliation method refers to adding MoS2 powder materials with a layered structure into different solvents or solvents containing a certain dispersant, and then using physical forces to destroy the van der Waals force between the two-dimensional material layers to achieve the purpose of preparing a single-layer MoS2. The yield of single-layer MoS2 prepared by mechanical exfoliation is low, and the structure of the obtained single-layer MoS2 is often destroyed. The ion intercalation method mainly embeds the intercalator into the MoS2 layer, increases its interlayer spacing, reduces the van der Waals force between the layers, thereby achieving the separation and exfoliation of the layers, and then obtains multi-layer or single-layer MoS2 nanosheets by washing and drying. This method has high efficiency and good product quality, but the operation is complicated and the preparation time is slightly longer, and it cannot be prepared on a large scale. The liquid phase ultrasonic method generally places MoS2 in a suitable solvent to destroy the cohesive energy between adjacent layered crystals, and then uses ultrasonic action to exfoliate it. After standing, take the upper clear liquid and dry it under vacuum conditions to obtain nanosheets. This method has a simple process, high efficiency, and does not require special equipment, but the product quality is relatively poor. Chemical vapor deposition refers to a preparation method that obtains products through chemical reactions. It mainly uses high temperature to vaporize the reactants into a gaseous state, and chemically reacts with each other in the gaseous state, and then deposits the products on the surface of a selected solid substrate to obtain nanosheets. Chemical vapor deposition is a relatively mature method for preparing nanosheets. Its main advantages are that the prepared products have high purity and good crystallization properties. Therefore, it is widely used in the production of single crystals, polycrystals, the development of new crystals, and the preparation of inorganic thin film materials. However, compared with other methods, this method has extremely stringent equipment requirements, and requires high temperatures during the reaction, which is costly and difficult to mass produce.
[0004] Therefore, it is particularly important to design a method for efficiently and quickly exfoliating MoS2 and keeping it in a flaky structure. The present invention utilizes ion intercalation to successfully obtain MoS2 in a flaky structure through a modified hydrothermal reaction. Summary of the invention
[0005] In order to overcome the shortcomings of the prior art, the present invention aims to provide a method for ion intercalation exfoliation of MoS2 to obtain a sheet structure. 2+ and Cs + As an intercalant, sodium carboxymethyl cellulose was used to increase the viscosity of the solution. During the hydrothermal reaction, high temperature accelerated the Zn 2+ and Cs + The reduction weakens the van der Waals force between MoS2 layers, which is conducive to the exfoliation of MoS2. The present invention provides a method for obtaining a flaky structure by ion intercalation exfoliation of MoS2, which comprises the following steps:
[0006] S1. Add 3-8 mol of CsCl, 5-12 mol of zinc acetylacetonate solution and 1-2 mol of sodium carboxymethyl cellulose into a 500 ml beaker and stir for 3-8 hours;
[0007] S2, adding 20-40 mol of multilayered MoS2 powder to the solution obtained in S1, and ultrasonicating for 1-3 hours to obtain a dispersion system of MoS2 powder;
[0008] S3, transfer the powder dispersion system obtained in S2 to a stainless steel high-pressure reactor, react at 250-330°C for 18-22h, cool to room temperature and then take out;
[0009] S4. Pour the solution in the stainless steel reactor obtained in S3 into a beaker, and ultrasonically clean it with 0.1-0.3M HCl for 20-40 minutes. Then replace the HCl with deionized water and continue ultrasonic treatment for 1-2 hours. Then, vacuum filter the filtrate and dry it in an oven at 60-80°C to obtain the exfoliated single-layer flaky MoS2.
[0010] Preferably, 3 mol of CsCl is selected in step S1.
[0011] Preferably, 8 mol of zinc acetylacetonate is selected in step S1.
[0012] Preferably, the stirring time in step S1 is 5 hours.
[0013] Preferably, the ultrasonic time in step S2 is 2 hours.
[0014] Preferably, 32 mol of multilayered MoS2 powder is added in step S2.
[0015] Preferably, the reaction temperature in step S3 is 300°C.
[0016] Preferably, the reaction time in step S3 is 20 h.
[0017] Preferably, the HCl selected in step S4 is 0.2M.
[0018] The beneficial effects of applying the present invention are:
[0019] 1. The present invention provides a method for ion intercalation exfoliation of MoS2 flake structure, using hydrothermal high temperature intercalation of Zn 2+ and Cs +This helps to reduce the contact angle and increase the number of interlayer electrons. The reduction in contact angle is due to the increase in hydrophilicity caused by the change in surface groups, and the increase in the number of electrons comes from the change in reaction intermediates and valence states. The reduction in contact angle helps the solvent molecules to enter the interlayer during ultrasonic peeling, and the increase in the number of interlayer electrons increases the repulsive force between the layers, improves the peeling efficiency, and thus helps ultrasonic peeling.
[0020] 2. The present invention adds sodium carboxymethyl cellulose, which increases the viscosity of the solution and is conducive to the dispersion of MoS2. At the same time, high temperature will produce a synergistic effect with sodium carboxymethyl cellulose, which is conducive to reducing its contact angle, thereby increasing the number of interlayer electrons, which is more conducive to the exfoliation of MoS2.
[0021] 3. Vacuum filtration after hydrothermal treatment will remove excess Zn in the solution. 2+ and Cs + , thereby protecting the MoS2 crystal structure. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is the SEM image of MoS2 prepared in Example 1 of the present invention.
[0023] Figure 2 This is the SEM image of MoS2 prepared in Comparative Example 1 of the present invention.
[0024] Figure 3 BET diagram of MoS2 prepared in Example 1 and Comparative Example 2 of the present invention.
[0025] Figure 4 BET diagram of MoS2 prepared in Example 2, Comparative Example 3 and Comparative Example 4 of the present invention.
[0026] Figure 5 This is the XRD pattern of MoS2 prepared in Example 3 of the present invention.
[0027] Figure 6 The XRD pattern of MoS2 prepared in comparative example 5 of the present invention. DETAILED DESCRIPTION
[0028] The following describes the embodiments of the present invention by specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that the following embodiments and features in the embodiments can be combined with each other without conflict.
[0029] Example 1
[0030] S1. Add 3 mol of CsCl, 12 mol of zinc acetylacetonate solution and 2 mol of sodium carboxymethyl cellulose into a 500 ml beaker and stir for 3 h.
[0031] S2, adding 20 mol of multilayered MoS2 powder to the solution obtained in S1, and ultrasonicating for 1 h to obtain a dispersion system of MoS2 powder;
[0032] S3, transfer the powder dispersion system obtained in S2 to a stainless steel high-pressure reactor, react at 250°C for 18 hours, cool to room temperature, and then take out;
[0033] S4. Pour the solution in the stainless steel reactor obtained in S3 into a beaker, and ultrasonically clean it with 0.1M HCl for 20 minutes. Then replace the HCl with deionized water and continue ultrasonic treatment for 1 hour. Then, vacuum filter the filtrate and dry it in an oven at 60°C to obtain the exfoliated single-layer flaky MoS2.
[0034] Comparative Example 1: In step S1, 3 mol of CsCl and 12 mol of zinc acetylacetonate are not added, and the rest is the same as in Example 1.
[0035] Comparative Example 2: No sodium carboxymethyl cellulose was added in step S1, and the rest was the same as in Example 1.
[0036] Figure 1 The SEM image of the MoS2 sample prepared in Example 1 is shown in Figure 1. Figure 1 It can be seen that after the MoS2 sample is hydrothermally treated, Zn 2+ and Cs + After intercalation, a micrometer-scale lamellar structure was prepared. Figure 2 This is the SEM image of the MoS2 sample microstructure prepared in Comparative Example 1. Figure 2 The MoS2 before exfoliation is a micron-scale lamellar structure with a large thickness and irregular morphology. The difference between the two is that 3 mol of CsCl and 12 mol of zinc acetylacetonate release Zn during the hydrothermal process. 2+ and Cs + , Zn 2+ and Cs + is reduced and embedded in MoS2 to form (Zn / Cs) x MoS2, Zn 2+ and Cs + There is a synergistic effect between them. The embedding of the two weakens the van der Waals force between MoS2 layers, thereby achieving the purpose of exfoliating MoS2 and making MoS2 thinner. The thinner MoS2 sheet structure will expose more active sites, which is of great significance for catalysis, batteries and optics.
[0037] Figure 3 The specific surface area comparison diagram of MoS2 samples prepared by Example 1 and Comparative Example 2 is shown in Table 1. Figure 3 It can be seen that the specific surface area of Example 1 is slightly larger than that of Comparative Example 2. This is because sodium carboxymethyl cellulose is not added in Comparative Example 2. The use of sodium carboxymethyl cellulose will significantly increase the viscosity of the solution, which effectively prevents the agglomeration of MoS2 nanosheets and is conducive to reducing the contact angle and improving the peeling effect.
[0038] Table 1 Comparison of specific surface areas of MoS2 samples prepared in Example 1 and Comparative Example 2
[0039]
[0040] Example 2
[0041] S1. Add 8 mol of CsCl, 5 mol of zinc acetylacetonate solution and 1 mol of sodium carboxymethyl cellulose into a 500 ml beaker and stir for 8 h.
[0042] S2, adding 40 mol of multilayered MoS2 powder to the solution obtained in S1, and ultrasonicating for 3 h to obtain a dispersion system of MoS2 powder;
[0043] S3, transfer the powder dispersion system obtained in S2 to a stainless steel high-pressure reactor, react at 330°C for 22h, cool to room temperature and then take out;
[0044] S4. Pour the solution in the stainless steel reactor obtained in S3 into a beaker, and ultrasonically clean it with 0.3M HCl for 40 minutes. Then replace the HCl with deionized water and continue ultrasonic treatment for 2 hours. Then, vacuum filter the filtrate and dry it in an oven at 80°C to obtain the exfoliated single-layer flaky MoS2.
[0045] Comparative Example 3: The reaction temperature in step S3 is 180°C, and the rest is the same as in Example 2.
[0046] Comparative Example 4: The heating temperature in step S3 is 350°C, and the rest is the same as in Example 2.
[0047] Figure 4 The specific surface area comparison diagram of MoS2 samples prepared at different temperatures is shown in Figure 2. Figure 4It can be known that when the heating temperature is 330°C in Example 2, the prepared exfoliated MoS2 sample has the largest specific surface area. When the hydrothermal temperature is 350°C in Comparative Example 4, the specific surface area of the prepared exfoliated MoS2 sample is lower than that of Example 2. This is because the high temperature in the hydrothermal reaction will accelerate the reduction of ions and weaken the interlayer van der Waals force of MoS2. The appropriate temperature helps to reduce the contact angle of MoS2 and increase the number of interlayer electrons, making it easy to exfoliate MoS2. In Comparative Example 3, the temperature is relatively low, which is not enough to achieve the best exfoliation effect of MoS2. However, in Comparative Example 4, when the hydrothermal reaction temperature is 350°C, the excessively high temperature will carbonize sodium carboxymethyl cellulose, which is not enough to prevent MoS2 from agglomerating. Therefore, it shows that there is an obvious synergistic relationship between the high temperature of the hydrothermal reaction and sodium carboxymethyl cellulose, and both are conducive to weakening the number of interlayer electrons of MoS2, making it easy to exfoliate.
[0048] Table 1 Comparison of specific surface areas of MoS2 samples prepared in Example 2, Comparative Example 3 and Comparative Example 4
[0049]
[0050] Example 3
[0051] S1. Add 5 mol of CsCl, 8 mol of zinc acetylacetonate solution and 2 mol of sodium carboxymethyl cellulose into a 500 ml beaker and stir for 6 hours.
[0052] S2, adding 35 mol of multilayered MoS2 powder to the solution obtained in S1, and ultrasonicating for 2 h to obtain a MoS2 powder dispersion system;
[0053] S3, transfer the powder dispersion system obtained in S2 to a stainless steel high-pressure reactor, react at 300°C for 20h, cool to room temperature and then take out;
[0054] S4. Pour the solution in the stainless steel reactor obtained in S3 into a beaker, and ultrasonically clean it with 0.2M HCl for 35 minutes. Then replace the HCl with deionized water and continue ultrasonic treatment for 1.5 hours. Then, vacuum filter the filtrate and dry it in an oven at 70°C to obtain the exfoliated single-layer flaky MoS2.
[0055] Comparative Example 5: No vacuum filtration is performed in step S4, and the rest is the same as in Example 3.
[0056] At the same time, the present invention also explores whether vacuum filtration has an effect on the exfoliation of MoS2 flake structures. Figure 5 The XRD diffraction pattern of the exfoliated MoS2 flake structure prepared in Example 3 of the present invention is shown in FIG. Figure 5It can be seen that the characteristic diffraction pattern of molybdenum disulfide remains unchanged, indicating that the crystal structure of MoS2 is not destroyed after hydrothermal intercalation, and there is no doping of intercalation agent. In comparative example 5, without vacuum filtration, XRD will show mixed peaks. Figure 6 This is the XRD pattern of the material prepared in Example 5 of the present invention. The peaks are marked with a dotted line. This shows that vacuum filtration in the present invention can remove excess unreacted Zn in the solution. 2+ and Cs + .
[0057] In summary, the present invention discloses a method for obtaining a sheet structure by ion intercalation exfoliation of MoS2, using CsCl and zinc acetylacetonate as intercalation agents, which are mainly responsible for providing Zn 2+ and Cs + , thus entering the interlayer of MoS2. In addition, the use of sodium carboxymethyl cellulose will increase the viscosity of the solution to prevent the agglomeration of MoS2, and at the same time it will be easier to open the interlayer structure of MoS2, making it easier to peel off. During the high temperature process of the hydrothermal reaction, the high temperature will accelerate the Zn 2+ and Cs + The reduction of Zn in the solution weakens the van der Waals force between MoS2 layers. At the same time, high temperature will produce a synergistic effect with sodium carboxymethyl cellulose, which is conducive to reducing its contact angle, thereby increasing the number of electrons between layers and being more conducive to the exfoliation of MoS2. Vacuum filtration after hydrothermal treatment will remove excess Zn in the solution. 2+ and Cs + , thereby protecting the crystal structure of MoS2.
[0058] The above-mentioned embodiments only express the specific implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the protection scope of the present invention. It should be pointed out that, for those skilled in the art, without departing from the concept of the present invention, any other changes, modifications, substitutions, combinations, simplifications made without departing from the spirit and principle of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A method for obtaining a flaky structure by ion intercalation exfoliation of MoS2, characterized in that: Specifically, the method comprises the following steps: S1, putting 3-8 mol of CsCl, 5-12 mol of zinc acetylacetonate solution and 1-2 mol of sodium carboxymethyl cellulose into a 500 ml beaker and stirring for 3-8 hours; S2, adding 20-40 mol of multilayer MoS2 powder into the solution obtained in S1, and ultrasonically treating for 1-3 hours to obtain a dispersion system of MoS2 powder; S3, transferring the powder dispersion system obtained in S2 to a stainless steel high-pressure reactor, reacting at a temperature of 250-330° C. for 18-22 hours, and cooling to room temperature before taking out; S4, pouring the solution in the stainless steel reactor obtained in S3 into a beaker, ultrasonically cleaning with 0.1-0.3 M HCl for 20-40 minutes, replacing HCl with deionized water and continuing ultrasonic treatment for 1-2 hours, followed by vacuum filtration, and drying the filtrate in an oven at 60-80° C. to obtain a single-layer flaky MoS2 after exfoliation.
2. The method for obtaining a flaky structure by ion intercalation exfoliation of MoS2 according to claim 1, characterized in that: In step S1, 3 mol of CsCl is selected.
3. A method for obtaining a flaky structure by ion intercalation exfoliation of MoS2 according to claim 1 or 2, characterized in that: In step S1, 8 mol of zinc acetylacetonate is selected.
4. The method for obtaining a flaky structure by ion intercalation exfoliation of MoS2 according to claim 3, characterized in that: The stirring time in step S1 is 5 h.
5. The method for obtaining a flaky structure by ion intercalation exfoliation of MoS2 according to claim 1, characterized in that: The ultrasonic time in step S2 is 2 hours.
6. The method for obtaining a flaky structure by ion intercalation exfoliation of MoS2 according to claim 5, characterized in that: In step S2, 32 mol of multilayered MoS2 powder is added.
7. The method for obtaining a flaky structure by ion intercalation exfoliation of MoS2 according to claim 1, characterized in that: The reaction temperature in step S3 is 300°C.
8. The method for obtaining a flaky structure by ion intercalation exfoliation of MoS2 according to claim 1, characterized in that: The reaction time in step S3 is 20 h.
9. The method for obtaining a flaky structure by ion intercalation exfoliation of MoS2 according to claim 1, characterized in that: The HCl used in step S4 is 0.2M.