Aerated concrete and preparation method thereof

By utilizing scrap materials from aerated concrete and phosphogypsum, combined with specific preparation processes, the problems of insufficient strength and low waste utilization rate of aerated concrete have been solved, resulting in the production of high-strength lightweight aerated concrete suitable for load-bearing walls and promoting environmentally friendly production.

CN115959879BActive Publication Date: 2024-11-22GUIZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211701519.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-28
Publication Date
2024-11-22
Estimated Expiration
2042-12-28

AI Technical Summary

Technical Problem

The low strength of aerated concrete limits its application in load-bearing walls, and the waste generated during the production process is not effectively utilized, affecting its promotion and environmental protection.

Method used

High-strength lightweight aerated concrete is prepared using scraps from aerated concrete and phosphogypsum as main raw materials, combined with foam stabilizers, surfactants and composite foaming agents, through a specific preparation process, including steps such as drying, ball milling, mixing, stirring, pouring and constant pressure curing.

Benefits of technology

It improves the compressive and flexural strength of aerated concrete, realizes the recycling of waste materials, and has lightweight, high strength, thermal insulation and sound absorption properties, meeting the requirements of green environmental protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115959879B_ABST
    Figure CN115959879B_ABST
Patent Text Reader

Abstract

The invention discloses a kind of aerated concrete and preparation method thereof, belong to the technical field of concrete, a kind of aerated concrete, its raw materials include the following components by weight: 200-280 parts of aerated concrete scraps, 150-170 parts of phosphogypsum, 80-120 parts of fly ash, 80-120 parts of cement, 40-80 parts of fluorite tailings, 40-60 parts of sand, 20-40 parts of slag powder, 0.05 parts of foam stabilizer, 0.2-0.6 parts of surfactant, 6-10 parts of composite foaming agent. The present invention reuses the scraps produced by producing concrete, mixes the waste with phosphogypsum, fly ash and the like with water, so that the waste produced by producing aerated concrete is recycled, the comprehensive utilization rate of industrial solid waste is improved, green and environmental protection, and a certain effect is played on the pollution and protection of the environment; the aerated concrete has higher compressive strength and lower dry density, so as to have the advantages of light weight, high strength, thermal insulation, sound absorption and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of concrete, in particular to aerated concrete and a preparation method thereof. Background Art

[0002] Aerated concrete is a material that is formed by the chemical reaction of calcium and silicon aggregates to form hydrothermal silicate CSH (B) and tobermorite crystals, which bind the "aggregate debris" together and form a lightweight porous concrete material together with the generated pores. Aerated concrete blocks are lightweight and porous, and have good thermal insulation, heat insulation and sound absorption properties. They are good thermal insulation and sound insulation materials, but their strength is generally not high, which hinders the widespread application and promotion of aerated concrete. Due to its large porosity, aerated concrete walls often have hollows and cracks, and cannot be used as load-bearing walls, which also affects the appearance and life of the wall.

[0003] The raw materials for producing aerated concrete are widely available, and industrial wastes such as sand, slag, phosphogypsum, and fly ash can be selected. It is in line with the national sustainable development strategy according to local conditions. The scraps of aerated concrete are the cutting residues produced by the cutting process, the mold collapse waste produced by the mold collapse, the casting waste and other semi-finished wastes in the manufacturing process. The discarding of these wastes will cause a lot of waste. Phosphogypsum is an industrial by-product produced by the production of phosphoric acid. Its properties can be changed by adding phosphogypsum to change its strength, bulk density, etc., and the current utilization rate is only 15%. The present invention uses aerated concrete scraps, phosphogypsum, etc. to prepare aerated concrete, turning waste into treasure, and improving the comprehensive utilization rate of solid waste. The aerated concrete obtained has a pore structure with good stability and a high strength grade, which is conducive to factory production and application. Summary of the invention

[0004] Based on the technical problems existing in the background technology, the present invention proposes an aerated concrete and a preparation method thereof. The purpose of the present invention can be achieved through the following technical solutions:

[0005] Aerated concrete, whose raw materials include the following components by weight: 200-280 parts of aerated concrete scraps, 150-170 parts of phosphogypsum, 80-120 parts of fly ash, 80-120 parts of cement, 40-80 parts of fluorite tailings, 40-60 parts of sand, 20-40 parts of slag powder, 0.05 parts of foam stabilizer, 0.2-0.6 parts of surfactant, and 6-10 parts of composite foaming agent.

[0006] Furthermore, the foam stabilizer is a foam stabilizer specially used for aerated concrete sold on the market.

[0007] Furthermore, the surfactant includes dodecyl dimethyl amine oxide, sodium dodecyl sulfonate, sodium tartrate, and betaine.

[0008] Furthermore, the composite foaming agent comprises aluminum powder and 99.9% tea polyphenols (analytical grade).

[0009] Furthermore, a method for preparing aerated concrete comprises the following preparation steps:

[0010] S1. Treatment of aerated concrete scraps: Dry the aerated concrete waste residue in a constant temperature drying oven at 80°C for 48 hours, and grind it in a planetary ball mill for a period of time to 55-75μm fine powder for later use;

[0011] S2. Treatment of other fillers: Dry phosphogypsum, fly ash, cement, fluorite tailings, sand and slag powder in a constant temperature drying oven for 6 hours, grind with a planetary ball mill to 55-75 μm fine powder for later use;

[0012] S3, prepare a composite foaming agent by taking 6-10 parts of aluminum powder and 1-5 parts of 99.9% tea polyphenols (analytical grade), mix and grind into 55-75 μm fine powder, and set aside;

[0013] S4, pouring the aerated concrete waste residue prepared in step S1, the filler prepared in step S2, the composite foaming agent, the foam stabilizer and the surfactant prepared in step S3 into a container and mixing them, adding the mixture into a mixer for stirring, and evenly mixing the mixed powder and the aqueous solution after stirring, and then pouring them into a mold for casting, and then putting them into an oven for standing and pre-curing after the casting is completed, and manually cutting the excess material on the mold after the foaming is completed.

[0014] S5. Finally, the preformed aerated concrete is transferred into an autoclave for constant pressure curing. The aerated concrete can be obtained by curing and forming.

[0015] Furthermore, in step S4, the rotation speed of the stirrer is 15 r / min, and the stirring time of the stirrer is 60-100 min.

[0016] Furthermore, the aqueous solution in step S4 is deionized water heated to about 50° C., and the water-cement ratios of the aqueous solution and the mixed powder when mixed in step S4 are: 0.55, 0.6, 0.63, 0.68, 0.7.

[0017] Furthermore, the size of the mold used for casting in step S4 is: 100mm*100mm*100mm.

[0018] Furthermore, in step S4, the temperature in the oven is 50° C., and the static pre-curing time is 8 h to 16 h.

[0019] Furthermore, the constant pressure curing selected in step S5 is to preheat the autoclave for 40 min, then evacuate the air in the autoclave to make the autoclave in a vacuum state, and keep the pressure in the autoclave constant at 1.15 MPa, and the constant pressure curing time is 8-12 h.

[0020] Beneficial effects of the present invention:

[0021] 1. The present invention reuses the scraps generated by concrete production, mixes the scraps with phosphogypsum, fly ash and water, so that the scraps generated by aerated concrete production can be recycled, thereby improving the comprehensive utilization rate of industrial solid waste, being green and environmentally friendly, and playing a certain role in environmental pollution and protection.

[0022] 2. The aerated concrete has high compressive strength and low dry density, thus having the advantages of light weight, high strength, thermal insulation, and sound absorption. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 The present invention is a flow chart of aerated concrete preparation. DETAILED DESCRIPTION

[0024] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] The present invention is further described below with reference to Examples and Comparative Examples.

[0026] Example 1

[0027] S1: Treatment of aerated concrete scraps: The aerated concrete waste residues were dried in a constant temperature drying oven at 80°C for 48 hours, and then ball-milled in a planetary ball mill for a period of time until they were ground into 55 μm fine powder for later use;

[0028] S2: Treatment of other fillers: Phosphogypsum, fly ash, cement, fluorite tailings, sand, and slag powder were dried in a constant temperature drying oven for 6 h, and then ground into 55 μm fine powder using a planetary ball mill for later use;

[0029] S3: Prepare a composite foaming agent by taking 6 parts of aluminum powder and 1 part of 99.9% tea polyphenols (analytical grade), mix and grind into 55 μm fine powder, and set aside;

[0030] S4: 200 parts of aerated concrete waste residue prepared in step S1, 150 parts of filler prepared in step S2, 6 parts of composite foaming agent prepared in step S3, 0.05 parts of foam stabilizer and 0.2 parts of surfactant are put into a container and mixed, and stirred at 15r / min for 60min in a mixer, and the mixed powder and aqueous solution are evenly mixed according to a water-cement ratio of 0.55, and then poured into a mold of 100mm*100mm*100mm, and placed in a 50℃ oven for pre-curing for 8h. After the foaming is completed, the excess material on the mold is manually cut.

[0031] S5: Finally, the preformed aerated concrete is transferred into an autoclave and cured at a constant pressure of 1.15 MPa for 8 hours to obtain aerated concrete after curing.

[0032] Example 2

[0033] S1. Treatment of aerated concrete scraps: The aerated concrete waste residues were dried in a constant temperature drying oven at 80°C for 48 hours, and then ball-milled in a planetary ball mill for a period of time until they were ground into 60μm fine powder for later use;

[0034] S2. Treatment of other fillers: Phosphogypsum, fly ash, cement, fluorite tailings, sand, and slag powder are dried in a constant temperature drying oven for 6 hours, and then ground into 60 μm fine powder using a planetary ball mill for later use;

[0035] S3, prepare a composite foaming agent by taking 7 parts of aluminum powder and 2 parts of 99.9% tea polyphenols (analytical grade), mix and grind into 60 μm fine powder, and set aside;

[0036] S4, 220 parts of aerated concrete waste residue prepared in step S1, 155 parts of fillers prepared in step S2, 7 parts of composite foaming agent prepared in step S3, 0.05 parts of foam stabilizer and 0.3 parts of surfactant are put into a container and mixed, and stirred at 15r / min for 70min in a mixer, and the mixed powder and aqueous solution are evenly mixed at a water-cement ratio of 0.6, and then poured into a mold of 100mm*100mm*100mm, and pre-cured in an oven at 50°C for 10h. After foaming, the excess material on the mold is manually cut.

[0037] S5. Finally, the preformed aerated concrete is transferred into an autoclave and cured at a constant pressure of 1.15 MPa for 9 hours. After curing and shaping, aerated concrete can be obtained.

[0038] Example 3

[0039] S1. Treatment of aerated concrete scraps: The aerated concrete waste residues were dried in a constant temperature drying oven at 80°C for 48 hours, and then ball-milled in a planetary ball mill for a period of time until they were ground into 65μm fine powder for later use;

[0040] S2. Treatment of other fillers: Phosphogypsum, fly ash, cement, fluorite tailings, sand, and slag powder are dried in a constant temperature drying oven for 6 hours, and then ground into 65 μm fine powder using a planetary ball mill for later use;

[0041] S3, taking 8 parts of aluminum powder and 3 parts of 99.9% tea polyphenols (analytical grade) to prepare a composite foaming agent, mixing and grinding to 65 μm fine powder, and setting aside;

[0042] S4, 240 parts of aerated concrete waste residue prepared in S1, 160 parts of filler prepared in step S2, 8 parts of composite foaming agent prepared in step S3, 0.05 parts of foam stabilizer and 0.4 parts of surfactant are put into a container and mixed, and stirred for 80 min at 15 r / min in a mixer, and the mixed powder and aqueous solution are mixed evenly according to a water-cement ratio of 0.63, and then poured into a mold of 100mm*100mm*100mm, and placed in a 50°C oven for pre-curing for 12 hours. After the foaming is completed, the excess material on the mold is manually cut

[0043] S5. Finally, the preformed aerated concrete is transferred into an autoclave and cured at a constant pressure of 1.15 MPa for 10 hours. After curing and shaping, aerated concrete can be obtained.

[0044] Example 4

[0045] S1. Treatment of aerated concrete scraps: The aerated concrete waste residues were dried in a constant temperature drying oven at 80°C for 48 hours, and then ball-milled in a planetary ball mill for a period of time until they were ground into 70 μm fine powder for later use;

[0046] S2. Treatment of other fillers: Phosphogypsum, fly ash, cement, fluorite tailings, sand, and slag powder are dried in a constant temperature drying oven for 6 hours, and then ground into 70 μm fine powder using a planetary ball mill for later use;

[0047] S3, taking 9 parts of aluminum powder and 4 parts of 99.9% tea polyphenols (analytical grade) to prepare a composite foaming agent, mixing and grinding to 70 μm fine powder, and setting aside;

[0048] S4, put 260 parts of aerated concrete waste residue prepared in step S1, 165 parts of filler prepared in step S2, 9 parts of composite foaming agent prepared in step S3, 0.05 parts of foam stabilizer and 0.5 parts of surfactant into a container and mix them, stir them at 15r / min for 90min in a mixer, mix the mixed powder and aqueous solution evenly according to a water-cement ratio of 0.68, pour them into a mold of 100mm*100mm*100mm, and stand them in a 50℃ oven for pre-curing for 14h. After foaming, manually cut the excess material on the mold.

[0049] S5. Finally, the preformed aerated concrete is transferred into an autoclave and cured at a constant pressure of 1.15 MPa for 11 hours. After curing and shaping, aerated concrete can be obtained.

[0050] Example 5

[0051] S1. Treatment of aerated concrete scraps: The aerated concrete waste residues were dried in a constant temperature drying oven at 80°C for 48 hours, and then ball-milled in a planetary ball mill for a period of time until they were ground into 75 μm fine powder for later use;

[0052] S2. Treatment of other fillers: Phosphogypsum, fly ash, cement, fluorite tailings, sand, and slag powder are dried in a constant temperature drying oven for 6 hours, and then ground into 75 μm fine powder using a planetary ball mill for later use;

[0053] S3, taking 10 parts of aluminum powder and 5 parts of 99.9% tea polyphenols (analytical grade) to prepare a composite foaming agent, mixing and grinding to 75 μm fine powder, and setting aside;

[0054] S4, put 280 parts of aerated concrete waste residue prepared in step S1, 170 parts of filler prepared in step S2, 10 parts of composite foaming agent prepared in step S3, 0.05 parts of foam stabilizer and 0.6 parts of surfactant into a container and mix them, stir them at 15r / min for 100min in a mixer, mix the mixed powder and aqueous solution evenly according to a water-cement ratio of 0.7, pour them into a mold of 100mm*100mm*100mm, and stand in an oven at 50℃ for pre-curing for 16h. After foaming, manually cut the excess material on the mold.

[0055] S5. Finally, the preformed aerated concrete is transferred into an autoclave and cured at a constant pressure of 1.15 MPa for 12 hours. After curing and shaping, aerated concrete can be obtained.

[0056] Table 1. Raw material addition table of Examples 1-5

[0057]

[0058] Comparative Example

[0059] Comparative Example 1

[0060] The difference between Comparative Example 1 and Example 1 is that no aerated concrete scraps are added to the raw materials of Comparative Example 1, and the rest are consistent with Example 1.

[0061] Comparative Example 2

[0062] The difference between Comparative Example 2 and Example 1 is that tea polyphenols are not added to the composite foaming agent in the raw materials of Comparative Example 2, and the rest are consistent with Example 1.

[0063] Performance Testing

[0064] 1. Compressive strength: Referring to the detection method disclosed in GB / T11969-2008 "Test method for performance of autoclaved aerated concrete", test pieces with a size of 100 mm*100 mm*100 mm were prepared, and the compressive strength of aerated concrete Examples 1-5 and Comparative Examples 1-2 was tested using a pressure testing machine. The results are shown in Table 2.

[0065] 2. Flexural strength: Referring to the detection method disclosed in GB / T11969-2008 "Test method for performance of autoclaved aerated concrete", test pieces with a size of 100 mm*100 mm*400 mm were made, and the flexural strength of aerated concrete Examples 1-5 and Comparative Examples 1-2 were tested. The results are shown in Table 2.

[0066] 3. Dry density: Referring to the detection method disclosed in GB / T11969-2008 "Test method for performance of autoclaved aerated concrete", test pieces with a size of 100 mm*100 mm*100 mm were prepared. Aerated concrete Examples 1-5 and Comparative Examples 1-2 were dried at (105±5)°C to a constant weight, and their dry densities were calculated. The results are shown in Table 2.

[0067] Table 2 Comparison of performance of aerated concrete products in different embodiments and comparative examples

[0068] Sample No. Compressive strength / MPa Intensity Level Flexural strength / MPa Dry density (kg / m3) Example 1 9.2 A10.0 5.2 493 Example 2 8.9 A10.0 5.2 520 Example 3 7.3 A7.5 5.1 538 Example 4 9.3 A10.0 5.5 540 Example 5 9.1 A10.0 5.3 480 Comparative Example 1 4.2 A5.0 3.2 550 Comparative Example 2 8.9 A10.0 4.8 825

[0069] By comparing the performance results of Comparative Example 1 and Example 1, it can be seen that: when preparing aerated concrete, the compressive strength and flexural strength of the aerated concrete blocks prepared by adding aerated concrete scraps in Example 1 are higher than the compressive strength and flexural strength of the aerated concrete prepared in Comparative Example 1. It can be seen that adding aerated concrete scraps to aerated concrete can effectively improve the compressive strength and flexural strength, and the compressive strength grade of the aerated concrete blocks prepared by adding aerated concrete scraps can reach above A7.5, which is conducive to factory production and promotion.

[0070] By comparing the performance results of Comparative Example 2 with those of Example 1, it can be seen that when preparing aerated concrete, if tea polyphenols are added to the foaming agent, the dry density of the prepared aerated concrete is lower than the dry density of the aerated concrete prepared without adding tea polyphenols to the foaming agent. The low dry density of the aerated concrete indicates that the pore structure in the aerated concrete block is more uniform and has good stability, which is conducive to factory production and promotion.

[0071] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0072] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.

Claims

1. Aerated concrete, characterized in that: The raw materials include the following components by weight: 200-280 parts of aerated concrete scraps, 150-170 parts of phosphogypsum, 80-120 parts of fly ash, 80-120 parts of cement, 40-80 parts of fluorite tailings, 40-60 parts of sand, 20-40 parts of slag powder, 0.05 parts of foam stabilizer, 0.2-0.6 parts of surfactant, and 6-10 parts of composite foaming agent; The composite foaming agent comprises aluminum powder and 99.9% analytically pure tea polyphenols.

2. The aerated concrete according to claim 1, characterized in that The foam stabilizer is a foam stabilizer specially used for aerated concrete sold on the market.

3. The aerated concrete according to claim 1, characterized in that The surfactant includes dodecyl dimethylamine oxide, sodium lauryl sulfonate, sodium tartrate and betaine.

4. The method for preparing aerated concrete according to claim 1, wherein: The method comprises the following preparation steps: S1. Treatment of aerated concrete scraps: Dry the aerated concrete scraps in a constant temperature drying oven at 80°C for 48 hours, and grind them in a planetary ball mill for a period of time until they are ground into 55-75μm fine powder for later use; S2. Treatment of other fillers: Dry phosphogypsum, fly ash, cement, fluorite tailings, sand, and slag powder in a constant temperature drying oven for 6 h, and grind them into 55-75 μm fine powder using a planetary ball mill for later use; S3, prepare a composite foaming agent by taking 6-10 parts of aluminum powder and 1-5 parts of 99.9% analytically pure tea polyphenols, mix and grind into 55-75 μm fine powder, and set aside; S4, pouring the aerated concrete waste residue prepared in step S1, the filler prepared in step S2, the composite foaming agent, the foam stabilizer, and the surfactant prepared in step S3 into a container and mixing them, adding the mixed powder into a blender for stirring, and after stirring evenly, mixing the mixed powder and the aqueous solution evenly, and then pouring it into a mold for casting. After the casting is completed, the mixture is placed in an oven for static pre-curing. After the foaming is completed, the excess material on the mold is manually cut; S5. Finally, the preformed aerated concrete is transferred into an autoclave for constant pressure curing. After curing and shaping, aerated concrete can be obtained.

5. A method for preparing aerated concrete according to claim 4, characterized in that: In step S4, the rotation speed of the stirrer is 15 r / min, and the stirring time of the stirrer is 60-100 min.

6. The method for preparing aerated concrete according to claim 4, wherein: The aqueous solution in step S4 is deionized water heated to about 50° C. The water-cement ratios when the aqueous solution and the mixed powder are mixed in step S4 are: 0.55, 0.6, 0.63, 0.68, and 0.

7.

7. The method for preparing aerated concrete according to claim 6, wherein: The size of the mold used for casting in step S4 is: 100mm*100mm*100mm.

8. The method for preparing aerated concrete according to claim 6, wherein: In step S4, the temperature in the oven is 50° C., and the pre-curing time is 8 h to 16 h.

9. The method for preparing aerated concrete according to claim 6, wherein: The constant pressure curing selected in step S5 is to preheat the autoclave for 40 minutes, then evacuate the air in the autoclave to make the autoclave in a vacuum state, and keep the pressure in the autoclave constant at 1.15 MPa. The constant pressure curing time is: 8-12 hours.