A tubular porous titanium-based electrocatalytic membrane and a preparation method thereof

By building a TiO2 nanoarray layer on a titanium mesh and sintering it to form a tubular porous titanium-based electrocatalytic membrane with a regular and ordered pore structure, the problem of insufficient mechanical strength and small catalytic area of ​​traditional titanium-based membrane materials has been solved, and the treatment of organic pollutants in water has been achieved. Efficient removal and industrial application.

CN115970516BActive Publication Date: 2024-10-29DALIAN MARITIME UNIVERSITY
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310063243.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-18
Publication Date
2024-10-29
Estimated Expiration
2043-01-18

AI Technical Summary

Technical Problem

Traditional titanium-based electrocatalytic membrane materials have problems such as insufficient mechanical strength, uneven pore size distribution, and small effective catalytic area, resulting in low removal efficiency of organic pollutants in water.

Method used

A tubular porous titanium-based electrocatalytic membrane with a titanium mesh as the basic framework is used. By constructing a TiO2 nanoarray layer on the titanium mesh and performing a sintering process, a membrane material with a regular and ordered pore structure is formed. The catalyst is evenly distributed throughout the membrane skeleton. Improve mechanical strength and catalytic activity.

Benefits of technology

It improves the mechanical strength and catalytic efficiency of the membrane, achieves efficient removal of trace organic pollutants in water, has controllable pore size distribution, and is suitable for large-scale production and application.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention discloses a tubular porous titanium-based electrocatalytic membrane and a preparation method thereof, belonging to the technical field of new membrane materials. The method comprises: (1) using a porous titanium mesh as a raw material, constructing a TiO2 nano-array layer on the porous titanium mesh grid, and obtaining a porous titanium mesh loaded with a titanium-based oxide catalyst layer; (2) rolling the porous titanium mesh loaded with the catalyst layer into a tubular structure and fixing it; (3) sintering the fixed rolled titanium mesh under an inert gas or reducing gas atmosphere to obtain a tubular porous titanium-based electrocatalytic membrane; the tubular porous titanium-based electrocatalytic membrane can be used for deep treatment of low-concentration organic pollutants in water. The porous titanium-based electrocatalytic membrane prepared by the present invention can make up for the deficiencies in the mechanical strength of the membrane body, the membrane pore size distribution, etc. of the existing powder sintered titanium-based membrane materials, and the problem of the small effective catalytic area of ​​the existing catalytic membrane, and has the advantages of simple preparation process, high yield, and controllable precision, which is conducive to large-scale production and promotion and application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of novel membrane materials, and in particular relates to a tubular porous titanium-based electrocatalytic membrane and a preparation method thereof. Technical Background

[0002] With the rapid development of industry and the explosive growth of population, water pollution caused by industrial wastewater and municipal sewage has become increasingly serious, among which the pollution caused by soluble organic pollutants is particularly widespread. Membrane separation technology has been widely used in the treatment of urban and industrial wastewater because of its simple process and convenient operation. However, traditional membrane separation technology has two main disadvantages: (1) The membrane is easily affected by membrane fouling during long-term operation; (2) During the membrane separation process, pollutants are only enriched and no chemical degradation occurs. Electrocatalytic membrane technology is a new water treatment technology that combines membrane separation and electrocatalytic oxidation. Under the action of an external low-voltage electric field, it can enhance the membrane separation process, alleviate membrane fouling, and generate strong oxidizing free radicals to achieve online degradation of organic pollutants. It shows good application prospects in the field of organic pollutant removal in water.

[0003] The electrocatalytic membrane materials reported so far mainly include porous titanium membranes, titanium suboxide membranes, and carbon-based membrane materials. Among them, titanium metal is an anode electrocatalytic material with excellent performance, which has the advantages of stable physical and chemical properties, corrosion resistance, good electrochemical stability, and good conductivity. In recent years, it has received widespread attention in the field of electrocatalytic membranes. At present, common titanium-based membrane materials include porous flat membranes and tubular membranes. In our previous patent, we invented an asymmetric hollow fiber titanium-based catalytic membrane (202111008514.8). These titanium-based membrane materials are all made of titanium metal powder as raw material, formed by pressure molding or dry-wet phase conversion molding, and then sintered at high temperature. The pore structure is formed by the accumulation of powder particles, with small regularity and uneven distribution; and because the membrane matrix is ​​sintered by powder, the strength of the membrane matrix is ​​determined by the degree of sintering and adhesion of the titanium powder particles, and the mechanical strength of the membrane body is somewhat insufficient, especially for thin and small membrane materials. In addition, whether it is a flat plate, tubular or hollow fiber membrane, the catalyst is loaded on the basis of the base membrane. The catalyst is mainly loaded on the membrane surface and is less distributed inside the membrane pores. Therefore, the effective catalytic area on the membrane is small. Summary of the invention

[0004] The purpose of the present invention is to provide a tubular porous titanium-based electrocatalytic membrane and a preparation method thereof which can be used for deep treatment of trace organic pollutants in water with simple process and controllable precision, so as to improve the problems of insufficient mechanical strength, uneven pore size distribution, small effective catalytic area, etc.

[0005] The specific technical solution adopted by the present invention is as follows:

[0006] On the one hand, the present invention provides a tubular porous titanium-based electrocatalytic membrane, which includes a tubular conductive membrane substrate with a titanium mesh as a basic frame and a titanium-based oxide array catalyst layer supported on the tubular conductive membrane grid structure.

[0007] Preferably, the catalytic layer in the titanium-based catalytic membrane is TiO 2 The nanoarray or non-stoichiometric titanium oxide nanoarray layer is obtained by gas reduction / metal titanium reduction during high temperature treatment.

[0008] Preferably, the outer diameter of the tubular porous titanium-based electrocatalytic membrane is 1 to 200 mm, the average membrane pore diameter is 0.05 to 50 μm, and the porosity is 20% to 80%.

[0009] On the other hand, the present invention provides a method for preparing the above tubular porous titanium-based electrocatalytic membrane, comprising the following steps:

[0010] (1) Using porous titanium mesh as raw material, TiO 2 Nano-array layer, to obtain a porous titanium mesh loaded with a titanium-based oxide catalyst layer;

[0011] (2) rolling the porous titanium mesh carrying the catalyst layer into a compact tubular structure and fixing it;

[0012] (3) sintering the fixed rolled titanium mesh in an inert gas or reducing gas atmosphere to obtain a tubular porous titanium-based electrocatalytic membrane;

[0013] Preferably, in step (1), TiO 2 The specific method of the nanoarray layer is: using a porous titanium mesh as an anode and a graphite electrode, a platinum electrode, a metal titanium or a stainless steel electrode as a cathode, TiO is grown on the porous titanium mesh grid structure by an anodic oxidation method. 2 The titanium mesh of the nano-array layer is 40 to 500 meshes; after the reaction is completed, the nano-array layer is ultrasonically cleaned in deionized water to remove impurities, and the surface-loaded TiO 2 Porous titanium mesh for the nanoarray catalytic layer.

[0014] As a further preference, the electrolyte composition used is calculated by mass percentage as follows: NH 4 A mixed solution of F (0.25-5wt%), deionized water (0.1-30wt%) and ethylene glycol (balance); an oxidation voltage of 10-80V; and an oxidation time of 1-300min.

[0015] Preferably, the specific method of rolling the titanium mesh in step (2) is: cutting the porous titanium mesh carrying the catalytic layer into a desired size (e.g., a rectangle), setting the parameters of a thin plate rolling machine, placing the titanium mesh into the rolling machine and rolling it into a dense and compact tubular structure, and then fixing the tubular structure by fasteners or spot welding to obtain a tubular precursor film;

[0016] As a further preference, the working pressure of the hydraulic system of the rolling trigger is 0.2-16 MPa; the speed of the plate rolling machine is 0.1-100 m / min, among which the preferred rolling speed is 0.3-2 m / min; the inner diameter of the rolled tubular precursor film is 0.5-180 mm, and the wall thickness is 0.1-50 mm.

[0017] Preferably, the specific method of sintering the tubular porous titanium membrane in step (3) is: the porous tubular precursor membrane prepared in step (2) is sintered by a programmed temperature method to obtain a tubular porous titanium-based electrocatalytic membrane.

[0018] As a further preference, the sintering treatment atmosphere is a mixture of one or more gases selected from argon, nitrogen, and hydrogen; the heating program is as follows: the heating rate is 0.1 to 20°C / min, the temperature is increased to 500 to 700°C within 1 to 2 hours at this rate, the temperature is kept at this rate for 1 to 2 hours, the temperature is then increased to 800 to 1600°C within 30 to 90 minutes, the temperature is kept at this rate for 1 to 8 hours, and the temperature is finally naturally cooled to room temperature to obtain a tubular porous titanium-based electrocatalytic membrane;

[0019] The tubular porous titanium-based electrocatalytic membrane prepared by the present invention is composed of multiple layers of ordered titanium mesh stacked together, presenting a regular and ordered porous structure. The fine control of the membrane pore structure can be achieved by adjusting the number of titanium meshes, the number of titanium mesh layers, the thickness of the catalyst layer and the sintering process. Since the catalyst is pre-constructed on the raw titanium mesh and then rolled to obtain the catalyst membrane, the catalyst layer is evenly distributed in the entire skeleton of the prepared tubular titanium-based catalyst membrane. Among them, when the sintering atmosphere is a reducing atmosphere, or the sintering temperature is higher than 1300°C, the catalyst layer of the obtained tubular porous titanium-based electrocatalytic membrane is composed of TiO 2 The non-stoichiometric titanium oxide nanoarrays were obtained by partial reduction of the nanoarrays, while the pre-constructed TiO nanoarrays were retained under other conditions. 2 Nanoarray catalytic layer.

[0020] The tubular porous titanium-based electrocatalytic membrane prepared as above can be used for deep treatment of water containing low concentration of organic pollutants, for example, for deep treatment of micro-polluted water containing low concentration (0.01-50ppm) of antibiotics, environmental hormones, phenols, etc., and the working voltage range is 1.5-20V.

[0021] The present invention provides a method for preparing a tubular porous titanium-based electrocatalytic membrane. Since the raw material of the membrane material is a titanium mesh with a mesh structure, the mechanical strength of the membrane is greater than that of a conventional powder sintered titanium membrane material. Since the catalyst is loaded in the matrix of the entire catalytic membrane, it has more catalytic active sites and a larger active surface area than the conventional surface loading method, and has a higher electrocatalytic activity, and has a higher removal efficiency for organic pollutants in water. In addition, its pore size distribution is regular and orderly, and the membrane pore size, membrane tube size, membrane layer thickness, etc. can all be more accurately regulated. The porous titanium-based electrocatalytic membrane prepared by the present invention can make up for the deficiencies in the mechanical strength of the membrane body, the membrane pore size distribution, etc. of the existing powder sintered titanium-based membrane materials, and the problem of a small effective catalytic area of ​​the existing catalytic membrane, and has the advantages of a simple preparation process, a high yield, and controllable precision, which is conducive to large-scale production and promotion and application.

[0022] Beneficial Effects

[0023] (1) The tubular porous titanium-based electrocatalytic membrane provided by the present invention has higher mechanical strength and larger active surface area than the porous metal electrocatalytic membrane prepared by traditional methods, high catalytic efficiency, and broader application prospects.

[0024] (2) The membrane pore structure of the tubular porous titanium-based electrocatalytic membrane provided by the present invention is regular and adjustable, the entire preparation process is carried out in a stable environment, the method is simple, and can meet industrial requirements.

[0025] (3) The tubular porous titanium-based electrocatalytic membrane provided by the present invention has high removal efficiency for micro-polluting organic matter in water and will not introduce secondary pollution. DETAILED DESCRIPTION

[0026] The following non-limiting embodiments may enable a person skilled in the art to more fully understand the present invention, but are not intended to limit the present invention in any way.

[0027] Example 1

[0028] A 200-mesh plain woven titanium mesh (length × width 10 × 6 cm) was used as the anode and a graphite rod was used as the cathode. The mixture was oxidized in a 0.25 wt% ammonium fluoride, 10 wt% deionized water ethylene glycol solution for 45 min, and the voltage was set to 30 V. After the reaction, the mixture was ultrasonically cleaned for 20 s to remove impurities and obtain a TiO-loaded 2 Porous titanium mesh for the nanoarray catalytic layer.

[0029] The working pressure of the hydraulic system of the plate rolling machine is set to 0.5 MPa, and the rolling speed is set to 0.5 m / min; the porous titanium mesh loaded with the catalytic layer is placed in the plate rolling machine and rolled into a tubular structure with a diameter of 5 mm and a wall thickness of 0.5 mm, and both ends are fixed by spot welding; the fixed tubular structure is sintered in a tubular furnace with argon as the sintering atmosphere, and the temperature is raised to 600°C at 5°C / min and kept for 1 h, and then continued to be raised to 1000°C at 5°C / min and kept for 1 h, and then naturally cooled to room temperature to obtain a tubular porous titanium-based electrocatalytic membrane.

[0030] The tubular porous titanium-based electrocatalytic membrane successfully prepared in this embodiment has an average equivalent diameter of membrane pores of 3.50 μm and a porosity of 67.2%. The tubular porous titanium-based electrocatalytic membrane is used as the anode and stainless steel is used as the cathode to treat water containing phenol micro-contamination with a concentration of 10 ppm. When the working voltage is 0 V and 2.5 V, the removal rates of phenol are 8.5% and 99.8% respectively.

[0031] Example 2

[0032] A 300-mesh twill woven titanium mesh (length × width: 30 × 10 cm) was used as the anode and stainless steel was used as the cathode. The mixture was oxidized in a 0.5 wt% ammonium fluoride, 20 wt% deionized water ethylene glycol solution for 30 min at a voltage of 40 V. After the reaction, the mixture was ultrasonically cleaned for 25 s to remove impurities and obtain a TiO-loaded 2 Porous titanium mesh for the nanoarray catalytic layer.

[0033] The working pressure of the hydraulic system of the plate rolling machine is set to 1 MPa, and the rolling speed is set to 0.3 m / min; the porous titanium mesh loaded with the catalytic layer is placed in the plate rolling machine and rolled into a tubular structure with a diameter of 20 mm and a wall thickness of 3.0 mm, and fixed with fasteners; the fixed tubular structure is sintered in a tubular furnace with a sintering atmosphere of nitrogen, and the temperature is raised to 600°C at 3°C / min and kept for 2 h, and then continued to be raised to 1100°C at 3°C / min and kept for 2 h, and then naturally cooled to room temperature to obtain a tubular porous titanium-based electrocatalytic membrane.

[0034] The tubular porous titanium-based electrocatalytic membrane successfully prepared in this embodiment has an average equivalent diameter of membrane pores of 1.80 μm and a porosity of 60.5%. The tubular porous titanium-based electrocatalytic membrane is used as the anode and the graphite plate is used as the cathode to treat water with a concentration of 5 ppm of tetracycline micro-contamination. When the working voltage is 0 V and 3.0 V, the removal rates of tetracycline are 6.2% and 100%, respectively.

[0035] Example 3

[0036] A 450-mesh contrast woven titanium mesh (length × width 50 × 8 cm) was used as the anode and stainless steel was used as the cathode. The mixture was oxidized in a 0.25 wt% ammonium fluoride, 20 wt% deionized water ethylene glycol solution for 40 min at a voltage of 50 V. After the reaction was completed, the mixture was ultrasonically cleaned for 30 s to remove impurities and obtain a TiO-loaded 2 Porous titanium mesh for the nanoarray catalytic layer.

[0037] The working pressure of the hydraulic system of the plate rolling machine is set to 0.5 MPa, and the rolling speed is set to 0.5 m / min; the porous titanium mesh loaded with the catalytic layer is placed in the plate rolling machine and rolled into a tubular structure with a diameter of 20 mm and a wall thickness of 3.8 mm, and both ends are fixed by spot welding; the fixed tubular structure is sintered in a tubular furnace with a sintering atmosphere of a mixture of 95% nitrogen and 5% hydrogen, and the temperature is raised to 600°C at 5°C / min and kept for 1 h, and then continued to rise to 1000°C at 2°C / min and kept for 3 h, and then naturally cooled to room temperature to obtain a tubular porous titanium-based electrocatalytic membrane.

[0038] The tubular porous titanium-based electrocatalytic membrane successfully prepared in this embodiment has an average equivalent diameter of membrane pores of 1.05 μm and a porosity of 55.2%. The tubular porous titanium-based electrocatalytic membrane is used as the anode and the titanium plate is used as the cathode to treat water with a concentration of 3 ppm of bisphenol A micro-contamination. When the working voltage is 0 V and 2.5 V, the removal rates of bisphenol A are 7.6% and 99.9%, respectively.

[0039] Example 4

[0040] A 325 mesh plain woven titanium mesh (length × width 8 × 8 cm) was used as the anode and a titanium sheet was used as the cathode. The titanium sheet was oxidized in a 0.5 wt% ammonium fluoride, 10 wt% deionized water ethylene glycol solution for 60 min at a voltage of 45 V. After the reaction, the titanium sheet was ultrasonically cleaned for 20 s to remove impurities and a TiO-loaded titanium sheet was obtained. 2 Porous titanium mesh for the nanoarray catalytic layer.

[0041] The working pressure of the hydraulic system of the plate rolling machine is set to 0.6 MPa, and the plate rolling speed is 1.0 m / min; the porous titanium mesh loaded with the catalytic layer is placed in the plate rolling machine and rolled into a tubular structure with a diameter of 5 mm and a wall thickness of 1.0 mm, and both ends are fixed with clips; the fixed tubular structure is sintered in a tubular furnace with a sintering atmosphere of a mixture of 97% argon and 3% hydrogen, and the temperature is raised to 600°C at 5°C / min and kept for 1 h, and then continued to rise to 1050°C at 1°C / min and kept for 2 h, and then naturally cooled to room temperature to obtain a tubular porous titanium-based electrocatalytic membrane.

[0042] The tubular porous titanium-based electrocatalytic membrane successfully prepared in this embodiment has an average equivalent diameter of membrane pores of 1.62 μm and a porosity of 43.2%. The tubular porous titanium-based electrocatalytic membrane is used as the anode and the titanium sheet is used as the cathode to treat water with a concentration of 15 ppm of micro-contamination containing sulfamethoxazole. When the working voltage is 0 V and 2.0 V, the removal rates of sulfamethoxazole are 3.6% and 100%, respectively.

Claims

1. A tubular porous titanium-based electrocatalytic membrane, characterized in that: The tubular porous titanium-based electrocatalytic membrane comprises a tubular conductive membrane substrate with a titanium mesh as a basic frame and a titanium-based oxide array catalytic layer supported on the tubular conductive membrane grid structure; The method for preparing the tubular porous titanium-based electrocatalytic membrane comprises the following steps: (1) Using a porous titanium mesh as a raw material, constructing a TiO2 nanoarray layer on the porous titanium mesh grid to obtain a porous titanium mesh loaded with a titanium-based oxide catalyst layer; (2) rolling a porous titanium mesh loaded with a titanium-based oxide catalyst layer into a tubular structure and fixing it; (3) sintering the fixed rolled titanium mesh in an inert gas or reducing gas atmosphere to obtain a tubular porous titanium-based electrocatalytic membrane; The steps of constructing a TiO2 nano-array layer on a titanium mesh grid structure include: using a porous titanium mesh as an anode, growing a TiO2 nano-array layer on the porous titanium mesh grid structure by an anodic oxidation method; after the reaction is completed, ultrasonic cleaning is performed in water to remove impurities, thereby obtaining a porous titanium mesh with a surface-loaded TiO2 nano-array catalytic layer; wherein the electrolyte used is a mixed solution of NH4F, water and ethanol, and in terms of mass percentage: NH4F is 0.25-5%, water is 0.1-30% and ethylene glycol is the balance; The specific method of sintering the tubular porous titanium film is as follows: the porous tubular precursor film prepared in step (2) is subjected to a sintering treatment by a programmed temperature rising method to obtain a tubular porous titanium-based electrocatalytic film; The tubular porous titanium-based electrocatalytic membrane is stacked with multiple layers of ordered titanium meshes loaded with catalytic layers, presenting a regular and ordered porous structure; the catalytic layer is a TiO2 nanoarray or a non-stoichiometric titanium oxide nanoarray layer obtained by gas reduction or metal titanium reduction of the TiO2 nanoarray during high-temperature heat treatment.

2. The tubular porous titanium-based electrocatalytic membrane according to claim 1, characterized in that: The tubular porous titanium-based electrocatalytic membrane can achieve fine control of its membrane pore structure by adjusting the number of titanium meshes, the number of titanium mesh layers, the thickness of the catalyst layer and the sintering process.

3. The tubular porous titanium-based electrocatalytic membrane according to claim 1, characterized in that: The outer diameter of the tubular porous titanium-based electrocatalytic membrane is 1-200 mm, the average membrane pore diameter is 0.05-50 μm, and the porosity is 20%-80%.

4. The tubular porous titanium-based electrocatalytic membrane according to claim 1, characterized in that: The mesh number of the titanium mesh is 40 to 500 meshes, and the weaving mode of the titanium mesh is one of plain weave, twill weave and contrast weave.

5. The tubular porous titanium-based electrocatalytic membrane according to claim 1, characterized in that: In the step of constructing a TiO2 nano-array layer on the titanium mesh grid structure, the oxidation voltage is 10 to 80 V; and the oxidation time is 1 to 300 min.

6. The tubular porous titanium-based electrocatalytic membrane according to claim 1, characterized in that: The specific method of the titanium mesh rolling forming is: cutting the porous titanium mesh carrying the catalytic layer, setting the parameters of the thin plate rolling machine, putting the titanium mesh into the rolling machine and rolling it into a dense and compact tubular structure, and then fixing the tubular structure by fasteners or spot welding to obtain a tubular precursor film; The working pressure of the hydraulic system of the plate rolling machine is 0-16 MPa; the speed of the plate rolling machine is 0.1-100 m / min; the inner diameter of the rolled tubular precursor film is 0.5-180 mm, and the wall thickness is 0.1-50 mm.

7. The method for preparing a tubular porous titanium-based electrocatalytic membrane according to claim 1, characterized in that: The specific method of sintering the tubular porous titanium film is that the sintering atmosphere is a mixture of one or more gases selected from argon, nitrogen, hydrogen and carbon monoxide; The heating program is as follows: the heating rate is 0.1-20°C / min, the temperature is increased to 500-700°C within 1-2 hours, kept warm for 1-2 hours, then the temperature is increased to 800-1600°C within 30-90 minutes, kept warm for 1-8 hours, and finally cooled naturally to room temperature to obtain a tubular porous titanium-based electrocatalytic membrane.

8. The tubular porous titanium-based electrocatalytic membrane according to claim 1, characterized in that: The tubular porous titanium-based electrocatalytic membrane can be applied to the deep treatment of low-concentration organic pollutants in water.

Citation Information

Patent Citations

  • Asymmetric hollow fiber titanium-based membrane and its preparation method

    CN113546526B

  • Preparation method for mesoporous titanium dioxide thin film

    CN102586836A