A ZSM-5 molecular sieve composite material and its preparation method and application, and a method for preparing methane

By encapsulating nickel oxide and manganese additives in the ZSM-5 molecular sieve pore, the problem of Ni-based catalyst in the hydrogenation of CO2 is solved, and efficient and stable catalytic effect is achieved, which is suitable for industrial applications.

CN115970743BActive Publication Date: 2024-11-26INST OF COAL CHEM CHINESE ACAD OF SCI
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310193660.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-03
Publication Date
2024-11-26
Estimated Expiration
2043-03-03

AI Technical Summary

Technical Problem

The existing Ni-based catalysts have problems of rapid sintering, agglomeration and carbon accumulation in the CO2 hydrogenation and methane reaction, resulting in catalyst deactivation and the high cost of precious metal catalysts, which limits their application.

Method used

Using ZSM-5 molecular sieve composite material, nickel oxide and manganese additives are encapsulated in the all-silicon ZSM-5 molecular sieve pores, the pore domain effect is used to prevent metal sites from sintering and agglomeration, and hydrothermal is carried out through organic amine ligand protection. Crystallization to prepare a highly active and stable catalyst.

Benefits of technology

It has achieved high CO2 conversion rate, high methane selectivity and yield, high catalytic activity and strong stability. After 100 hours of reaction, the catalyst has no obvious inactivation, which is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115970743B_ABST
    Figure CN115970743B_ABST
Patent Text Reader

Abstract

The present invention provides a ZSM-5 molecular sieve composite material and a preparation method and application thereof, and a methane preparation method, and relates to the technical field of catalysts. The ZSM-5 molecular sieve composite material provided by the present invention comprises an all-silicon ZSM-5 molecular sieve and nickel oxide and manganese additives encapsulated in the pores of the all-silicon ZSM-5 molecular sieve, wherein Ni is CO 2 The main active site for methanogenesis, while Mn is an important structural additive. The addition of manganese additive can weaken the strong interaction between Ni and the molecular sieve framework, promote the reduction of NiO to produce more Ni, and improve the methane selectivity and CO 2 Moreover, the ZSM-5 molecular sieve composite material provided by the present invention can make full use of the pore confinement effect of the all-silicon ZSM-5 molecular sieve to prevent the metal sites from sintering and agglomerating during the reaction, thereby greatly improving the catalytic stability of the ZSM-5 molecular sieve composite material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of catalysts, and in particular to a ZSM-5 molecular sieve composite material, a preparation method and application thereof, and a method for preparing methane. Background Art

[0002] With the extensive use of fossil resources, excess CO2 is released into the atmosphere, causing the CO2 content in the atmosphere to increase year by year. As of 2022, the global atmospheric CO2 concentration has reached 417ppm, causing serious environmental problems such as greenhouse effect, seawater acidification, and sea level rise. CO2 is also an important carbon-containing resource, which can be catalytically converted into high-value-added chemicals such as methane, methanol, low-carbon olefins and aromatics through hydrogenation. Among them, methane is not only the main component of natural gas, which can be directly used as a fuel, but also an important carrier of hydrogen energy. Compared with synthetic methanol, low-carbon olefins and aromatics, CO2 methanation shows a higher conversion rate and target product selectivity, and the reaction can be carried out at a lower pressure, so it is easier to scale up.

[0003] Precious metal catalysts such as Rh, Ru, Pt and Pd show very high activity in CO2 methanation reaction. However, these precious metals are expensive, which limits their practical application. In contrast, cheap and abundant Ni-based catalysts are widely used in CO2 hydrogenation to methane. However, existing Ni-based catalysts are prone to sintering and agglomeration during the reaction; in addition, they are also prone to quickly produce a large amount of carbon deposits, resulting in rapid deactivation of the catalyst. Siakavelas et al. (Siakavelas GI, Charisiou ND, AlKhoori S, et al. Highly selective and stable nickel catalysts supported on ceria promoted with Sm2O3, Pr2O3 and MgO for the CO2 methanation reaction [J]. Applied Catalysis B: Environmental, 2021, 282: 119562.) reported a Ni / MgO-CeO2 catalyst. Although the methane selectivity was close to 100%, its CO2 conversion rate was only 43%, which was low. Fan et al. (Fan Q, Li S, Zhang L, et al. Regulation of product distribution in CO2 hydrogenation by modifying Ni / CeO2 catalysts[J]. Journal of Catalysis, 2022, 414: 53-63.) developed Ni / CeO2 and Ni-Mn / CeO2 catalysts. In the CO2 methanation reaction, the CO2 conversion rate was 23.4% and 38.2%, and the methane selectivity was 78.4% and 89.0%. The CO2 conversion rate was low and the two catalysts began to deactivate after 30 hours of reaction and had poor stability.

[0004] Molecular sieves are widely used as metal carriers due to their unique pore structure. Compared with carriers such as zirconium oxide, silicon oxide, and aluminum oxide, molecular sieves have a larger surface area and a three-dimensional porous structure, which can better disperse metals. Some studies have shown that encapsulating metals in the pores of molecular sieves and utilizing the confinement effect of the pores can effectively prevent the rapid sintering and agglomeration of metal sites. For example, Yu et al. (Qiming Sun, Ning Wang, Qiyuan Fan et al. Subnanometer Bimetallic Platinum–Zinc Clusters in Zeolites for Propane Dehydrogenation [J]. Angew. Chem. Int. Ed. 59 (2020) 19450-19459) encapsulated Pd and Zn bimetallics in the pores of ZSM-5 molecular sieves, which significantly alleviated the rapid agglomeration of Pd and Zn during the reaction process and showed high stability in the propane dehydrogenation reaction. Although traditional metal-molecular sieve encapsulated catalysts show high stability, the overly strong interaction between metal and molecular sieve is not conducive to the reduction of metal sites, resulting in low catalytic activity. Summary of the invention

[0005] In view of this, the object of the present invention is to provide a ZSM-5 molecular sieve composite material and its preparation method and application. The ZSM-5 molecular sieve composite material provided by the present invention catalyzes the CO2 hydrogenation to CH4 reaction, has high CO2 conversion rate, high methane selectivity and yield, high catalytic activity and strong catalytic stability.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] The invention provides a ZSM-5 molecular sieve composite material, comprising an all-silicon ZSM-5 molecular sieve and nickel oxide and manganese additives encapsulated in pores of the all-silicon ZSM-5 molecular sieve.

[0008] Preferably, in the ZSM-5 molecular sieve composite material, the mass fraction of Ni element is 0.2-2.0%, and the mass fraction of Mn element is 0.05-1.0%.

[0009] The present invention provides a method for preparing the ZSM-5 molecular sieve composite material described in the above technical solution, comprising the following steps:

[0010] Mixing a water-soluble nickel source, a water-soluble manganese source, an organic amine ligand and water to obtain a Ni-Mn-ligand mixture precursor solution;

[0011] The Ni-Mn-ligand mixture precursor solution is mixed with the initial gel for synthesizing the all-silicon ZSM-5 molecular sieve, and then subjected to hydrothermal crystallization and calcination to obtain a ZSM-5 molecular sieve composite material.

[0012] Preferably, the molar ratio of Ni to Mn in the Ni-Mn-ligand mixture precursor solution is 1:(0.02-5.4), and the ratio of the total amount of Ni and Mn to the amount of organic amine ligand is 1:(20-100);

[0013] The organic amine ligand includes one or more of ethylenediamine, cyclohexylamine and cyclohexanediamine.

[0014] Preferably, the molar ratio of the effective ingredients SiO2, template and H2O in the initial gel for synthesizing the all-silicon ZSM-5 molecular sieve is 1:(0.2-0.8):(20-100).

[0015] Preferably, the hydrothermal crystallization temperature is 150-200° C. and the time is 40-120 h.

[0016] Preferably, the calcination temperature is 500-650° C. and the calcination time is 5-10 h.

[0017] The present invention provides the use of the ZSM-5 molecular sieve composite material described in the above technical solution or the ZSM-5 molecular sieve composite material prepared by the preparation method described in the above technical solution in catalyzing CO2 hydrogenation to produce CH4.

[0018] The present invention also provides a method for preparing methane, comprising the following steps: subjecting a CO2-H2 mixed gas to a catalytic hydrogenation reaction in the presence of a catalyst to obtain CH4; the catalyst is the ZSM-5 molecular sieve composite material described in the above technical scheme or the ZSM-5 molecular sieve composite material prepared by the preparation method described in the above technical scheme; and the catalyst is subjected to a reduction treatment before use.

[0019] Preferably, the volume ratio of H2 to CO2 in the CO2-H2 mixed gas is (1-8):1, and the space velocity of the CO2-H2 mixed gas is 1-100 L / (h·g); the temperature of the catalytic hydrogenation reaction is 300-450° C., the time is 10-500 h, and the pressure is 0.1-2.0 MPa;

[0020] The temperature of the reduction treatment is 400-700° C., the time is 1-8 hours, and the reducing agent used is hydrogen.

[0021] The present invention provides a ZSM-5 molecular sieve composite material, including an all-silicon ZSM-5 molecular sieve (denoted as x% Ni-y% Mn @ ZSM-5, wherein x% represents the mass fraction of Ni, and y% represents the mass fraction of Mn) and Ni and manganese additives encapsulated in the pores of the all-silicon ZSM-5 molecular sieve. In the ZSM-5 molecular sieve composite material provided by the present invention, Ni is the main active site for CO2 methanation, and Mn is an important structural additive. The addition of the manganese additive can weaken the strong interaction between the Ni substance and the molecular sieve framework, thereby promoting the reduction of NiO, producing more Ni, and improving the methane selectivity and CO2 conversion rate. At the same time, the ZSM-5 molecular sieve composite material prepared by the present invention belongs to a metal-molecular sieve encapsulated catalyst, which can make full use of the pore confinement effect of the all-silicon ZSM-5 molecular sieve to prevent the sintering and agglomeration of the metal (Ni and Mn) sites during the reaction process, thereby significantly improving the stability of the ZSM-5 molecular sieve composite material, and has a good application prospect in the catalytic carbon dioxide hydrogenation to prepare methane reaction. The test results of the embodiment show that the ZSM-5 molecular sieve composite material provided by the present invention is used for CO2 methanation reaction, with a methane selectivity of up to 98.86%, a CO2 conversion rate of up to 76.68%, and no obvious deactivation of the catalyst after 100 hours of reaction.

[0022] The present invention provides a method for preparing the ZSM-5 molecular sieve composite material described in the above technical solution, comprising the following steps: mixing a water-soluble nickel source, a water-soluble manganese source, an organic amine ligand and water to obtain a Ni-Mn-ligand mixture precursor solution; mixing the Ni-Mn-ligand mixture precursor solution with the initial gel synthesized from the all-silicon ZSM-5 molecular sieve, performing hydrothermal crystallization and then calcining to obtain the ZSM-5 molecular sieve composite material. The present invention performs hydrothermal crystallization in an environment of a soluble nickel source and a soluble manganese source solution protected by an organic amine ligand, and can encapsulate Ni-Mn in the pores of the all-silicon ZSM-5 molecular sieve. The preparation method of the ZSM-5 molecular sieve composite material provided by the present invention is simple to operate, has no secondary pollution, is green and environmentally friendly, has low production cost, and is suitable for industrial production and application. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 XRD spectrum of 0.90%Ni-0.39%Mn@ZSM-5 prepared in Example 1;

[0024] Figure 2 N2 adsorption-desorption curve of 0.90%Ni-0.39%Mn@ZSM-5 prepared in Example 1;

[0025] Figure 3 This is the SEM image of 0.90%Ni-0.39%Mn@ZSM-5 prepared in Example 1;

[0026] Figure 4 TEM image of 0.90%Ni-0.39%Mn@ZSM-5 prepared in Example 1;

[0027] Figure 5 This is a graph showing the stability results of the CO2 methanation reaction of 0.90% Ni-0.39% Mn@ZSM-5 prepared in Example 1. DETAILED DESCRIPTION

[0028] The invention provides a ZSM-5 molecular sieve composite material, comprising an all-silicon ZSM-5 molecular sieve and nickel oxide and manganese additives encapsulated in pores of the all-silicon ZSM-5 molecular sieve.

[0029] In the present invention, the mass fraction (x%) of Ni element in the ZSM-5 molecular sieve composite material is preferably 0.2-2.0%, more preferably 0.5-1.5%; the mass fraction (y%) of Mn element in the ZSM-5 molecular sieve composite material is preferably 0.05-1.0%, more preferably 0.1-0.5%; the manganese additive is preferably manganese oxide, more preferably MnO2. In the present invention, the nickel oxide is preferably NiO.

[0030] In the present invention, the particle size of the ZSM-5 molecular sieve composite material is preferably 10 to 60 meshes, more preferably 20 to 50 meshes. The present invention controls the particle size of the ZSM-5 molecular sieve composite material within the above range, which is conducive to better catalyzing the methanation reaction of CO2.

[0031] In the ZSM-5 molecular sieve composite material provided by the present invention, Ni is the main active site for CO2 methanation, Mn is an important structural additive, and the addition of manganese additive can weaken the strong interaction between Ni and the molecular sieve framework, thereby promoting the reduction of NiO, producing more Ni, and improving the selectivity of CH4 and CO2 conversion rate in the CO2 hydrogenation to CH4 reaction. At the same time, the ZSM-5 molecular sieve composite material provided by the present invention belongs to a metal-molecular sieve encapsulated catalyst, which can make full use of the pore confinement effect of the all-silicon ZSM-5 molecular sieve to prevent the sintering and agglomeration of metal sites during the reaction, thereby improving the stability of the catalyst.

[0032] The present invention provides a method for preparing the ZSM-5 molecular sieve composite material described in the above technical solution, comprising the following steps:

[0033] Mixing a water-soluble nickel source, a water-soluble manganese source, an organic amine ligand and water to obtain a Ni-Mn-ligand mixture precursor solution;

[0034] The Ni-Mn-ligand mixture precursor solution is mixed with the initial gel for synthesizing the all-silicon ZSM-5 molecular sieve, and then subjected to hydrothermal crystallization and calcination to obtain a ZSM-5 molecular sieve composite material.

[0035] Unless otherwise specified, the raw materials used in the present invention are all commercially available products.

[0036] The invention mixes a water-soluble nickel source, a water-soluble manganese source, an organic amine ligand and water to obtain a Ni-Mn-ligand mixture precursor solution.

[0037] In the present invention, the water-soluble nickel source is preferably a water-soluble nickel salt, more preferably comprises one or more of nickel nitrate, nickel sulfate and nickel chloride, further preferably nickel nitrate, nickel sulfate or nickel chloride.

[0038] In the present invention, the water-soluble manganese source is preferably a water-soluble manganese salt, more preferably includes one or more of manganese nitrate, manganese sulfate and manganese chloride, and further preferably is manganese nitrate, manganese sulfate or manganese chloride.

[0039] In the present invention, the organic amine ligand preferably includes one or more of ethylenediamine, cyclohexylamine and cyclohexyldiamine, and more preferably ethylenediamine, cyclohexylamine or cyclohexyldiamine.

[0040] In the present invention, the molar ratio of Ni and Mn in the Ni-Mn-ligand mixture precursor solution is preferably 1:(0.02-5.4), more preferably 1:(0.025-5.345), further preferably 1:(0.05-2), and most preferably 1:(0.07-1.07). In the present invention, the ratio of the total amount of Ni and Mn in the Ni-Mn-ligand mixture precursor solution to the amount of organic amine ligand is preferably 1:(20-100), more preferably 1:(30-80), and further preferably 1:(40-70). In the present invention, the organic amine ligand can serve as a synthesis template for the all-silicon ZSM-5 molecular sieve, and can also coordinate with metal (Ni, Mn) ions, thereby preventing the water-soluble nickel source and the water-soluble manganese source from precipitation reaction, and further helping Ni and Mn to be encapsulated into the molecular sieve pores.

[0041] In the present invention, the mixing is preferably: mixing a water-soluble nickel source, a water-soluble manganese source and water to obtain a Ni-Mn mixed solution; mixing the Ni-Mn mixed solution with an organic amine ligand to obtain a Ni-Mn-ligand mixture precursor solution. The present invention has no special restrictions on the amount of water used, as long as it can dissolve the water-soluble nickel source and the water-soluble manganese source; the water is preferably deionized water. In the present invention, the mixing temperature is preferably room temperature; the present invention has no special restrictions on the mixing method and time, as long as the raw materials can be mixed evenly, such as stirring and mixing.

[0042] After obtaining the Ni-Mn-ligand mixture precursor solution, the present invention mixes the Ni-Mn-ligand mixture precursor solution with the initial gel for synthesizing the all-silicon ZSM-5 molecular sieve, performs hydrothermal crystallization and then calcines to obtain the ZSM-5 molecular sieve composite material.

[0043] In the present invention, the molar ratio of the effective ingredient SiO2, template and H2O in the initial gel for synthesizing the all-silicon ZSM-5 molecular sieve is preferably 1: (0.2-0.8): (20-100), more preferably 1: (0.3-0.7): (30-90), and further preferably 1: (0.4-0.6): (40-80). In the present invention, the template preferably includes one or more of tetrapropylammonium hydroxide (TPAOH), tetraethylammonium hydroxide (TEAOH) and n-butylamine. In the present invention, the preparation method of the initial gel for synthesizing the all-silicon ZSM-5 molecular sieve preferably includes the following steps: mixing a silicon source, a template and water and aging them to obtain an initial gel for synthesizing the all-silicon ZSM-5 molecular sieve. In the present invention, the silicon source preferably includes one or more of tetramethyl orthosilicate, tetraethyl orthosilicate and tetrabutyl orthosilicate, more preferably tetramethyl orthosilicate, tetraethyl orthosilicate or tetrabutyl orthosilicate. In the present invention, the template is preferably used in the form of an aqueous template solution; the mass fraction of the aqueous template solution is preferably 15-50%, more preferably 20-45%. The present invention has no special restrictions on the mixing, as long as the raw materials can be mixed evenly; the mixing temperature is preferably room temperature; in an embodiment of the present invention, the mixing is preferably: the template aqueous solution is mixed with water until it is clear, and then the silicon source is added dropwise to mix; the present invention has no special restrictions on the dropping, and it can be added dropwise at a uniform speed. In the present invention, the aging temperature is preferably room temperature, and the aging time is preferably 1-5h, more preferably 2-4h, and further preferably 3h.

[0044] In the present invention, the temperature of the hydrothermal crystallization is preferably 150-200°C, more preferably 160-190°C, and further preferably 170-180°C; the time of the hydrothermal crystallization is preferably 40-120h, more preferably 50-100h, and further preferably 60-80h. The present invention performs hydrothermal crystallization in an environment of a soluble nickel source and a soluble manganese source solution protected by an organic amine ligand, and can encapsulate Ni-Mn in the pores of the all-silicon ZSM-5 molecular sieve.

[0045] After the hydrothermal crystallization is completed, the present invention preferably further comprises subjecting the obtained crystallization reaction liquid to solid-liquid separation, and drying the obtained solid product. The present invention has no particular limitation on the solid-liquid separation method, and a solid-liquid separation method well known to those skilled in the art may be used, such as centrifugal separation. The present invention has no special requirements for the drying conditions, and drying to constant weight may be performed using drying conditions well known in the art.

[0046] In the present invention, the calcination temperature is preferably 500-650°C, more preferably 530-620°C, and further preferably 550-600°C; the calcination holding time is preferably 5-10h, more preferably 6-9h, and further preferably 7-8h; the calcination atmosphere is preferably air.

[0047] After the calcination is completed, the present invention preferably further comprises tableting, crushing and screening the obtained calcined product in sequence to obtain a ZSM-5 molecular sieve composite material. The present invention has no particular limitation on the tableting, crushing and screening, and a ZSM-5 molecular sieve composite material with a particle size of 10 to 60 mesh can be obtained.

[0048] The present invention also provides the application of the ZSM-5 molecular sieve composite material described in the above technical solution in catalyzing CO2 hydrogenation to produce CH4.

[0049] The present invention also provides a method for preparing methane, comprising the following steps: subjecting a CO2-H2 mixed gas to a catalytic hydrogenation reaction in the presence of a catalyst to obtain CH4; the catalyst is the ZSM-5 molecular sieve composite material described in the above technical scheme or the ZSM-5 molecular sieve composite material prepared by the preparation method described in the above technical scheme; and the catalyst is subjected to a reduction treatment before use.

[0050] In the present invention, the temperature of the reduction treatment is preferably 400-700°C, more preferably 450-650°C, and further preferably 500-650°C; the time of the reduction treatment is preferably 1-8h, more preferably 2-7h, and further preferably 3-6h; the reducing agent used in the reduction treatment is preferably hydrogen.

[0051] In the present invention, the volume ratio of H2 to CO2 in the CO2-H2 mixed gas is preferably (1-8):1, more preferably (2-7):1, and further preferably (3-6):1. In the present invention, the space velocity of the CO2-H2 mixed gas is preferably 1-100 L / (h·g), more preferably 2-65 L / (h·g), and further preferably 4-30 L / (h·g).

[0052] In the present invention, the temperature of the catalytic hydrogenation reaction is preferably 300-450°C, more preferably 350-420°C, and further preferably 370-400°C; the time of the catalytic hydrogenation reaction is preferably 10-500h, more preferably 20-300h, and further preferably 40-200h; the total pressure of the catalytic hydrogenation reaction is preferably 0.1-2.0MPa, more preferably 0.1-1.5MPa, and further preferably 0.5-1.0MPa.

[0053] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0054] Example 1

[0055] 15.230 g of TPAOH aqueous solution (mass fraction of 25%) was added to 38.110 g of deionized water (H2O) and magnetically stirred until the solution was clear, 15.620 g of tetraethyl orthosilicate (TEOS) was added dropwise, and aged for 4 h at room temperature with stirring to obtain the initial gel for the synthesis of all-silicon ZSM-5 molecular sieve (molar composition of 35H2O:0.4TPAOH:1SiO2).

[0056] At room temperature, 0.200 g of nickel nitrate and 0.057 g of manganese nitrate were dissolved in 5 mL of deionized water, and then mixed with 2.420 g of ethylenediamine at room temperature. The obtained Ni-Mn-ligand mixture precursor solution was added to the initial gel for synthesis of the all-silicon ZSM-5 molecular sieve, stirred and mixed evenly, transferred to a 100 mL high-pressure reactor, hydrothermally crystallized at 170° C. for 48 h, centrifuged, and the obtained solid product was dried in an oven at 100° C. for 12 h, then placed in a muffle furnace, and calcined at 550° C. for 10 h in an air atmosphere, tableted, crushed, and sieved to obtain a ZSM-5 molecular sieve composite material with a particle size of 20 to 40 mesh (denoted as 0.90% Ni-0.39% Mn@ZSM-5).

[0057] Figure 1 The XRD spectrum of 0.90% Ni-0.39% Mn@ZSM-5 prepared in Example 1 is shown in FIG. Figure 1 It can be seen that the prepared ZSM-5 molecular sieve composite material exhibits typical diffraction peaks of ZSM-5 molecular sieve; and no diffraction peaks of nickel or manganese substances appear, indicating that the substances containing these metals are highly dispersed.

[0058] Figure 2The N2 adsorption-desorption curve of 0.90% Ni-0.39% Mn@ZSM-5 prepared in Example 1 is shown in FIG. Figure 2 It can be seen that the prepared ZSM-5 molecular sieve composite material has a higher specific surface area, which is beneficial to promote the high dispersion of nickel and manganese substances.

[0059] Figure 3 This is the SEM image of 0.90%Ni-0.39%Mn@ZSM-5 prepared in Example 1. Figure 3 It can be seen that the prepared ZSM-5 molecular sieve composite material has a typical hexagonal coffin-shaped morphology, and the grain size is 300-600nm.

[0060] Figure 4 TEM image of 0.90%Ni-0.39%Mn@ZSM-5 prepared in Example 1. Figure 4 It can be seen that no nickel or manganese substances were observed on the surface of the prepared ZSM-5 molecular sieve composite material, which further confirmed that the components containing these metals have a small grain size and are highly dispersed in the molecular sieve pores.

[0061] Example 2

[0062] A ZSM-5 molecular sieve composite material was prepared according to the method of Example 1, the only difference from Example 1 being that the amount of manganese nitrate used was 0.029 g, the amount of ethylenediamine used was 2.047 g, and hydrothermal crystallization was carried out at 180° C. for 40 h to obtain a ZSM-5 molecular sieve composite material (denoted as 0.90% Ni-0.20% Mn@ZSM-5).

[0063] Example 3

[0064] A ZSM-5 molecular sieve composite material was prepared according to the method of Example 1, the only difference from Example 1 being that the amount of manganese nitrate used was 0.0215 g, the amount of ethylenediamine used was 1.850 g, and hydrothermal crystallization was carried out at 160° C. for 72 h to obtain a ZSM-5 molecular sieve composite material (denoted as 0.90% Ni-0.10% Mn@ZSM-5).

[0065] Example 4

[0066] A ZSM-5 molecular sieve composite material was prepared according to the method of Example 1, the only difference from Example 1 being that the amount of manganese nitrate used was 0.007 g, the amount of ethylenediamine used was 1.752 g, and a ZSM-5 molecular sieve composite material (denoted as 0.90% Ni-0.05% Mn@ZSM-5) was obtained.

[0067] Example 5

[0068] A ZSM-5 molecular sieve composite material was prepared according to the method of Example 1, the only difference from Example 1 being that the amount of manganese nitrate used was 0.132 g, the amount of ethylenediamine used was 1.752 g, and a ZSM-5 molecular sieve composite material (denoted as 0.90% Ni-0.9% Mn@ZSM-5) was obtained.

[0069] Comparative Example 1

[0070] A ZSM-5 molecular sieve composite material was prepared according to the method of Example 1, the only difference from Example 1 being that no manganese nitrate was added, the amount of ethylenediamine used was 1.653 g, and a ZSM-5 molecular sieve composite material (recorded as 0.90% Ni@ZSM-5) was obtained.

[0071] Comparative Example 2

[0072] A ZSM-5 molecular sieve composite material was prepared according to the method of Example 1, the only difference from Example 1 being that 0.057 g of manganese nitrate was replaced by 0.0518 g of copper nitrate, and the amount of ethylenediamine used was 2.317 g, to obtain a ZSM-5 molecular sieve composite material (denoted as 0.90% Ni-0.39% Cu@ZSM-5).

[0073] Comparative Example 3

[0074] A ZSM-5 molecular sieve composite material was prepared according to the method of Example 1, the only difference from Example 1 being that 0.057 g of manganese nitrate was replaced by 0.049 g of indium nitrate, and the amount of ethylenediamine used was 2.021 g, to obtain a ZSM-5 molecular sieve composite material (denoted as 0.90% Ni-0.39% In@ZSM-5).

[0075] Comparative Example 4

[0076] A ZSM-5 molecular sieve composite material was prepared according to the method of Example 1, the only difference from Example 1 being that 0.057 g of manganese nitrate was replaced by 0.067 g of cobalt nitrate, and the amount of ethylenediamine used was 2.369 g, to obtain a ZSM-5 molecular sieve composite material (denoted as 0.90% Ni-0.39% Co@ZSM-5).

[0077] Comparative Example 5

[0078] A ZSM-5 molecular sieve composite material was prepared according to the method of Example 1, the only difference from Example 1 being that nickel nitrate was not added, the amount of ethylenediamine used was 0.768 g, and a ZSM-5 molecular sieve composite material (recorded as 0.39% Mn@ZSM-5) was obtained.

[0079] Application Example 1

[0080] Catalytic performance test of ZSM-5 molecular sieve composite materials prepared in Examples 1 to 5 and Comparative Examples 1 to 5

[0081] The ZSM-5 molecular sieve composite materials prepared in Examples 1 to 5 and Comparative Examples 1 to 5 were respectively subjected to reduction treatment at 600° C. in a hydrogen atmosphere for 4 hours to obtain an activated catalyst. A CO2-H2 mixed gas (H2:CO2 volume ratio=4:1) was introduced into a reactor containing the activated catalyst to perform a catalytic hydrogenation reaction to obtain methane.

[0082] The catalytic performance results of the ZSM-5 molecular sieve composite materials prepared in Examples 1 to 5 and Comparative Examples 1 to 5 under different catalytic hydrogenation reaction conditions are shown in Table 1:

[0083] Table 1 Catalytic performance of ZSM-5 molecular sieve composite materials prepared in Examples 1 to 5 and Comparative Examples 1 to 5

[0084]

[0085]

[0086] As shown in Table 1, the ZSM-5 molecular sieve composite material prepared by the present invention is used to catalyze the CO2 hydrogenation to CH4 reaction, and the CO2 conversion rate is 49.22-76.68%, the methane selectivity is 91.23-98.86%, and the methane yield is 44.92-75.81%. The CO2 conversion rate of the ZSM-5 molecular sieve composite material without manganese (Comparative Example 1) is only 31.47%, and the methane selectivity and yield are reduced to 66.34% and 20.88% respectively; when Mn is replaced by Cu, In and Co (Comparative Examples 2-4), the highest CO2 conversion rate is only 46.00%, and the methane selectivity and yield are not more than 84.01% and 38.64% respectively, indicating that the ZSM-5 molecular sieve composite material prepared by the present invention has excellent CO2 hydrogenation to CH4 catalytic performance. Moreover, the nickel-free ZSM-5 molecular sieve composite material (Comparative Example 5) has almost no catalytic activity for the hydrogenation of CO2 to CH4, indicating that nickel is the main active site for the hydrogenation of CO2 to methane, while manganese is an important additive.

[0087] Application Example 2

[0088] Catalytic stability test of the ZSM-5 molecular sieve composite material prepared in Example 1

[0089] Methane was prepared according to the method of Application Example 1, wherein the catalytic hydrogenation reaction conditions were: reaction temperature of 400°C, pressure of 0.1 MPa, CO2-H2 mixed gas space velocity of 12 L / (h·g), and the catalytic stability test results of the ZSM-5 molecular sieve composite material at different catalytic hydrogenation reaction times were as follows: Figure 5As shown, Con.(CO2) represents the CO2 conversion rate, Sel.(CH4) represents the methane selectivity, Sel.(CO) represents the carbon monoxide selectivity, CH4-STY represents the number of moles of methane generated per unit mole of Ni site per unit hour, and CO-STY represents the number of moles of carbon monoxide generated per unit mole of Ni site per unit hour. Figure 5 It can be seen that the ZSM-5 molecular sieve composite material prepared by the present invention is used to catalyze the carbon dioxide to methane reaction, and has high catalytic activity (high carbon dioxide conversion rate), high methane selectivity and yield, and low by-product carbon monoxide selectivity, and the ZSM-5 molecular sieve composite material has excellent stability in the carbon dioxide methanation reaction, and the ZSM-5 molecular sieve composite material has no obvious deactivation after 100 hours of reaction.

[0090] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A ZSM-5 molecular sieve composite material for catalyzing CO2 hydrogenation to CH4, characterized in that: It comprises an all-silicon ZSM-5 molecular sieve and nickel oxide and manganese additive encapsulated in the pores of the all-silicon ZSM-5 molecular sieve; the manganese additive is manganese oxide; In the ZSM-5 molecular sieve composite material, the mass fraction of Ni element is 0.2-2.0%, and the mass fraction of Mn element is 0.05-1.0%; The preparation method of the ZSM-5 molecular sieve composite material comprises the following steps: Mixing a water-soluble nickel source, a water-soluble manganese source, an organic amine ligand and water to obtain a Ni-Mn-ligand mixture precursor solution; The Ni-Mn-ligand mixture precursor solution is mixed with the initial gel for synthesizing the all-silicon ZSM-5 molecular sieve, and then subjected to hydrothermal crystallization and calcination to obtain a ZSM-5 molecular sieve composite material.

2. The method for preparing the ZSM-5 molecular sieve composite material according to claim 1, characterized in that: The following steps are involved: Mixing a water-soluble nickel source, a water-soluble manganese source, an organic amine ligand and water to obtain a Ni-Mn-ligand mixture precursor solution; The Ni-Mn-ligand mixture precursor solution is mixed with the initial gel for synthesizing the all-silicon ZSM-5 molecular sieve, and then subjected to hydrothermal crystallization and calcination to obtain a ZSM-5 molecular sieve composite material.

3. The preparation method according to claim 2, characterized in that: The molar ratio of Ni to Mn in the Ni-Mn-ligand mixture precursor solution is 1:(0.02-5.4), and the ratio of the total amount of Ni and Mn to the amount of organic amine ligand is 1:(20-100); The organic amine ligand includes one or more of ethylenediamine, cyclohexylamine and cyclohexanediamine.

4. The preparation method according to claim 2, characterized in that: The molar ratio of the effective components SiO2, template agent and H2O in the initial gel for synthesizing the all-silicon ZSM-5 molecular sieve is 1: (0.2-0.8): (20-100).

5. The preparation method according to claim 2, 3 or 4, characterized in that: The temperature of the hydrothermal crystallization is 150-200° C., and the time is 40-120 hours.

6. The preparation method according to claim 2, characterized in that: The calcination temperature is 500-650° C. and the calcination time is 5-10 hours.

7. Use of the ZSM-5 molecular sieve composite material according to claim 1 or the ZSM-5 molecular sieve composite material prepared by the preparation method according to any one of claims 2 to 6 in catalytic CO2 hydrogenation to CH4.

8. A method for preparing methane, characterized in that: The following steps are involved: The CO2-H2 mixed gas is subjected to a catalytic hydrogenation reaction in the presence of a catalyst to obtain CH4; the catalyst is the ZSM-5 molecular sieve composite material described in claim 1 or the ZSM-5 molecular sieve composite material prepared by the preparation method described in any one of claims 2 to 6; the catalyst is reduced before use.

9. The preparation method according to claim 8, characterized in that: The volume ratio of H2 to CO2 in the CO2-H2 mixed gas is (1-8):1, and the space velocity of the CO2-H2 mixed gas is 1-100 L / (h·g); the temperature of the catalytic hydrogenation reaction is 300-450° C., the time is 10-500 h, and the pressure is 0.1-2.0 MPa; The temperature of the reduction treatment is 400-700° C., the time is 1-8 hours, and the reducing agent used is hydrogen.

Citation Information

Patent Citations

  • Method for catalytic oxidation NO with ZSM-5 type molecular sieve as catalyst

    CN101259368A

  • Method for rapidly preparing Ni-ZSM-5 methanation catalyst

    CN105478157A

  • Metal-coated MFI hierarchical pore structure packaging catalyst and packaging method and application thereof

    CN111437870A

  • Selective hydrogenation molecular sieve material and preparation method thereof

    CN112742445A

  • Hierarchical pore ZSM-5 molecular sieve packaged Ni metal catalyst with micropores and mesopores as well as preparation method and application of hierarchical pore ZSM-5 molecular sieve packaged Ni metal catalyst

    CN115007197A