Pseudo-boehmite and preparation method thereof

By adjusting the pH value of aluminum nitrate solution and carrying out crystallization and aging reaction, the problem of insufficient pore volume and specific surface area of ​​existing pseudo-thin water-thin water-thin water-thin water-thin water-thin water-thin water-thin water-thin water-thin water-thin water-thin water-thin water-thin water-thin water-thin water-thin water-thin water-thin water-thin water-thin water-thin and exhaust gas purification catalyst.

CN115974115BActive Publication Date: 2024-11-15JIANGXI BAOHTEC NANO SCI CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202211609519.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-14
Publication Date
2024-11-15
Estimated Expiration
2042-12-14

AI Technical Summary

Technical Problem

The pore capacity of existing suprasilicon is not large enough and has a low specific surface area, making it difficult to meet the efficient needs of petroleum refining catalysts and exhaust purification catalysts.

Method used

By adding aqueous ammonia solution to the pH value to 7-10, performing a neutralization reaction, and then performing a crystallization reaction to convert precipitation into crystals, and then mixing it with water and additives for aging reaction to form a high specific surface area and Mass-thin water-aluminite with large pore volume.

Benefits of technology

The prepared phthalidae has a high specific surface area and large pore volume, with a pore volume of up to 2.91cm3/g and a specific surface area of ​​up to 552.6m2/g, meeting the requirements of efficient catalysts and adsorbents.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention belongs to the technical field of compound synthesis, and provides a pseudo-boehmite and a preparation method thereof, comprising the following steps: adding an ammonia solution to an aluminum nitrate solution, adjusting the pH value to 7-10, and performing a neutralization reaction to obtain a neutralized product; then performing a crystallization reaction on the neutralized product to obtain a crystallized product; and finally mixing the crystallized product with water and an auxiliary agent to perform an aging reaction to obtain pseudo-boehmite. The present invention first adds an ammonia solution to an aluminum nitrate solution to adjust the pH value to 7-10 to generate a pseudo-boehmite precipitate with a large pore size and a high pore volume, and then converts it into crystals through a crystallization reaction, and then mixes it with water and an auxiliary agent to perform an aging reaction to increase the crystal growth, thereby obtaining a pseudo-boehmite with a high specific surface area and a large pore volume. The results of the embodiment show that the pore volume of the pseudo-boehmite prepared by the present invention is 2.91cm 3 / g, specific surface area is 552.6m 2 / g.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of compound synthesis, and in particular to pseudo-boehmite and a preparation method thereof. Background Art

[0002] Pseudo-boehmite, also known as monohydrated alumina and pseudo-monohydrated soft boehmite, has high crystal purity, good peptizing performance and strong adhesiveness. It can be used as an adsorbent, binder or carrier for preparing petroleum refining catalysts, reforming catalysts and producing exhaust gas / automobile exhaust purification catalysts. Pseudo-boehmite is generally prepared by the following methods: (1) Alkali precipitation method, that is, neutralizing acidified aluminum salt with alkali. Alumina monohydrate is precipitated from the acidified aluminum salt solution with alkali, and then the pseudo-boehmite product is obtained through aging, washing, drying and other processes. This method is often called alkali precipitation; (2) Acid precipitation method, that is, strong acid or aluminum salt of strong acid neutralizes aluminate, firstly precipitates alumina monohydrate from aluminate solution with acid, and then the pseudo-boehmite product is obtained through aging, washing, drying and other processes. This method is often called acid precipitation; (3) Alkoxy aluminum hydrolysis method, alkoxy aluminum is hydrolyzed with water to generate alumina monohydrate, and then the pseudo-boehmite product is obtained through aging, filtering and drying. However, the pore volume of pseudo-boehmite prepared by the existing method is not large enough and the specific surface area is low. Summary of the invention

[0003] The object of the present invention is to provide a pseudo-boehmite and a preparation method thereof. The pseudo-boehmite prepared by the preparation method provided by the present invention has a high specific surface area and a large pore volume.

[0004] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0005] The present invention provides a method for preparing pseudo-boehmite, comprising the following steps:

[0006] (1) adding an aqueous ammonia solution to an aluminum nitrate solution, adjusting the pH value to 7 to 10, and performing a neutralization reaction to obtain a neutralized product;

[0007] (2) subjecting the neutralized product obtained in step (1) to a crystallization reaction to obtain a crystallized product;

[0008] (3) Mixing the crystallized product obtained in step (2) with water and an auxiliary agent, and subjecting the mixture to an aging reaction to obtain pseudo-boehmite.

[0009] Preferably, the concentration of the aluminum nitrate solution in step (1) is 20-30 g / L; and the mass concentration of the ammonia solution is 2-3%.

[0010] Preferably, the solvents of the aluminum nitrate solution and the ammonia solution in step (1) are independently aqueous alcohol solutions.

[0011] Preferably, the mass ratio of alcohol to water in the alcohol aqueous solution is (1-6):1.

[0012] Preferably, the neutralization reaction temperature in step (1) is 30-40° C., and the neutralization reaction time is 20-40 min.

[0013] Preferably, the temperature of the crystallization reaction in step (2) is 50-55° C., and the time of the crystallization reaction is 30-50 min.

[0014] Preferably, the auxiliary agent in step (3) includes one or more of (NH4)2CO3, NH4HCO3 and urea.

[0015] Preferably, the temperature of the aging reaction in step (3) is 60-70° C., and the time of the aging reaction is 50-80 min.

[0016] The present invention also provides pseudo-boehmite prepared by the preparation method described in the above technical solution.

[0017] Preferably, the pore volume of the pseudo-boehmite is 2.3 to 2.9 cm 3 / g, specific surface area is 500~550m 2 / g.

[0018] The present invention provides a method for preparing pseudo-boehmite, comprising the following steps: (1) adding an ammonia solution to an aluminum nitrate solution, adjusting the pH value to 7 to 10, and performing a neutralization reaction to obtain a neutralized product; (2) performing a crystallization reaction on the neutralized product obtained in step (1) to obtain a crystallized product; (3) mixing the crystallized product obtained in step (2) with water and an auxiliary agent, and performing an aging reaction to obtain pseudo-boehmite. The present invention first adds an ammonia solution to an aluminum nitrate solution to adjust the pH value to 7 to 10 to generate a pseudo-boehmite precipitate with a large pore size and a high pore volume, and then converts it into crystals through a crystallization reaction, and then mixes it with water and an auxiliary agent to perform an aging reaction to increase the crystal growth, thereby obtaining a pseudo-boehmite with a high specific surface area and a large pore volume. The results of the embodiment show that the pore volume of the pseudo-boehmite prepared by the preparation method provided by the present invention is 2.91cm 3 / g, specific surface area is 552.6m 2 / g. DETAILED DESCRIPTION

[0019] The present invention provides a method for preparing pseudo-boehmite, comprising the following steps:

[0020] (1) adding an aqueous ammonia solution to an aluminum nitrate solution, adjusting the pH value to 7 to 10, and performing a neutralization reaction to obtain a neutralized product;

[0021] (2) subjecting the neutralized product obtained in step (1) to a crystallization reaction to obtain a crystallized product;

[0022] (3) Mixing the crystallized product obtained in step (2) with water and an auxiliary agent, and subjecting the mixture to an aging reaction to obtain pseudo-boehmite.

[0023] The invention adds an ammonia solution to an aluminum nitrate solution, adjusts the pH value to 7-10, performs a neutralization reaction, and obtains a neutralized product. The invention adds an ammonia solution to an aluminum nitrate solution to adjust the pH value of the solution to 7-10, and generates a neutralized product pseudo-boehmite precipitate.

[0024] The present invention adjusts the pH value of the solution to 7 to 10, preferably adjusts the pH value of the solution to 8 to 9. The present invention ensures the smooth generation of pseudo-boehmite precipitation by adjusting the pH value of the solution to 7 to 10.

[0025] In the present invention, the concentration of the aluminum nitrate solution is preferably 20 to 30 g / L, more preferably 25 to 30 g / L. The present invention uses an aluminum nitrate solution in the above concentration range, which is conducive to obtaining a large-pore-diameter, high-pore-volume pseudo-boehmite precipitate, and further conducive to obtaining a high-pore-volume pseudo-boehmite.

[0026] In the present invention, the mass concentration of the ammonia solution is preferably 2-3%, more preferably 2.2-2.8%. The present invention uses an ammonia solution in the above concentration range, which is conducive to controlling the pH value of the solution.

[0027] In the present invention, the solvents of the aluminum nitrate solution and the ammonia solution are independently preferably alcohol aqueous solution. In the present invention, the mass ratio of alcohol to water in the alcohol aqueous solution is preferably (1-6):1, more preferably (3-6):1. In the present invention, the mass ratio of alcohol to water in the alcohol aqueous solution is preferably controlled within the above range, which is conducive to obtaining pseudo-boehmite with high specific surface area and large pore volume.

[0028] In the present invention, the alcohol is preferably one or more of methanol, ethanol, n-propanol and isopropanol, more preferably one or more of methanol, ethanol and isopropanol.

[0029] In the present invention, the temperature of the neutralization reaction is preferably 30-40°C, more preferably 30-35°C; the time of the neutralization reaction is preferably 20-40 minutes, more preferably 25-35 minutes. In the present invention, the temperature and time of the neutralization reaction are preferably controlled within the above ranges, which is conducive to the full progress of the neutralization reaction and the full use of the raw materials.

[0030] After obtaining the neutralized product, the present invention performs a crystallization reaction on the neutralized product to obtain a crystallized product. The present invention converts the neutralized product pseudo-boehmite precipitation into crystals through the crystallization reaction, so as to facilitate the subsequent process.

[0031] In the present invention, the temperature of the crystallization reaction is preferably 50-55°C, more preferably 52-55°C; the time of the crystallization reaction is preferably 30-50 minutes, more preferably 35-45 minutes. In the present invention, the temperature and time of the crystallization reaction are preferably controlled within the above ranges, which is conducive to the full conversion of pseudo-boehmite precipitate into crystals.

[0032] After the crystallization reaction is completed, the present invention preferably filters the product of the crystallization reaction to obtain a crystallized product. The present invention has no special limitation on the filtering operation, and a filtering technical solution well known to those skilled in the art can be used.

[0033] After obtaining the crystallized product, the present invention mixes the crystallized product with water and an auxiliary agent, performs an aging reaction, and obtains pseudo-boehmite. The present invention increases crystal growth by mixing the crystallized product with water and an auxiliary agent and performing an aging reaction, thereby obtaining pseudo-boehmite with a high specific surface area and a large pore volume.

[0034] The present invention has no special limitation on the mixing of the crystallization product with water and the auxiliary agent, and any mixing technical solution well known to those skilled in the art may be adopted.

[0035] In the present invention, the mass ratio of the crystallized product to the auxiliary agent is preferably (15-20): 1, and more preferably (18-20): 1. In the present invention, the mass ratio of the crystallized product to the auxiliary agent is preferably controlled within the above range, which is conducive to the formation of pseudo-boehmite with high specific surface area and large pore volume.

[0036] The present invention has no particular limitation on the amount of water used, as long as the amount of water can completely immerse the crystallized product and the auxiliary agent.

[0037] In the present invention, the auxiliary agent preferably includes one or more of (NH4)2CO3, NH4HCO3 and urea, and more preferably one or more of (NH4)2CO3 and NH4HCO3. The present invention has no particular limitation on the source of the auxiliary agent, and commercial products well known to those skilled in the art can be used.

[0038] In the present invention, the temperature of the aging reaction is preferably 60-70°C, more preferably 65-70°C; the time of the aging reaction is preferably 50-80 minutes, more preferably 55-70 minutes. In the present invention, the temperature and time of the aging reaction are preferably controlled within the above ranges, which is conducive to ensuring sufficient growth of crystals, thereby forming pseudo-boehmite with high specific surface area and large pore volume.

[0039] After the aging reaction is completed, the present invention preferably filters and dries the product of the aging reaction in sequence to obtain pseudo-boehmite. The present invention has no special limitation on the filtering and drying operations, and the filtering and drying technical solutions well known to those skilled in the art can be used. In the present invention, the drying temperature is preferably 80 to 90° C.; the drying time is preferably 50 to 70 minutes.

[0040] The invention adds an ammonia solution to an aluminum nitrate solution to adjust the pH value to 7-10 to generate pseudo-boehmite precipitation with large pore diameter and high pore volume, then converts it into crystals through a crystallization reaction, and then mixes it with water and an auxiliary agent to carry out an aging reaction to increase the growth of the crystals, thereby obtaining pseudo-boehmite with high specific surface area and large pore volume.

[0041] The present invention also provides pseudo-boehmite prepared by the preparation method described in the above technical solution. The pseudo-boehmite provided by the present invention has a high specific surface area and a large pore volume.

[0042] In the present invention, the pore volume of the pseudo-boehmite is preferably 2.3 to 2.9 cm 3 / g; the specific surface area of ​​the pseudo-boehmite is preferably 500 to 550m 2 / g.

[0043] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0044] Example 1

[0045] (1) adding an aqueous ammonia solution with a mass concentration of 2.5% to an aluminum nitrate solution with a concentration of 30 g / L, adjusting the pH value to 8, and then performing a neutralization reaction at 35° C. to obtain a neutralized product after 30 minutes; wherein the solvents of the aluminum nitrate solution and the aqueous ammonia solution are both methanol aqueous solution, and the mass ratio of methanol to water in the methanol aqueous solution is 5:1;

[0046] (2) subjecting the neutralized product obtained in step (1) to a crystallization reaction at 55° C. for 45 min, and then filtering to obtain a crystallized product;

[0047] (3) The crystallized product obtained in step (2) is mixed with water and NH4HCO3, and subjected to an aging reaction at 70°C for 60 minutes, and then filtered, and finally dried at 90°C for 60 minutes to obtain pseudo-boehmite; wherein the mass ratio of the crystallized product to NH4HCO3 is 18:1; and the pore volume of the pseudo-boehmite is 2.53 cm 3 / g, specific surface area is 527.3m 2 / g.

[0048] Example 2

[0049] (1) adding an aqueous ammonia solution with a mass concentration of 2.2% to an aluminum nitrate solution with a concentration of 25 g / L, adjusting the pH value to 9, and then performing a neutralization reaction at 40° C. to obtain a neutralized product after 20 minutes; wherein the solvents of the aluminum nitrate solution and the aqueous ammonia solution are both methanol aqueous solution, and the mass ratio of methanol to water in the methanol aqueous solution is 4:1;

[0050] (2) subjecting the neutralized product obtained in step (1) to a crystallization reaction at 50° C. for 40 min, and then filtering to obtain a crystallized product;

[0051] (3) The crystallized product obtained in step (2) is mixed with water and urea, subjected to an aging reaction at 65° C. for 70 min, filtered, and finally dried at 90° C. for 60 min to obtain pseudo-boehmite; wherein the mass ratio of the crystallized product to urea is 15:1; and the pore volume of the pseudo-boehmite is 2.38 cm 3 / g, specific surface area is 517.6m 2 / g.

[0052] Example 3

[0053] (1) adding an aqueous ammonia solution with a mass concentration of 2.2% to an aluminum nitrate solution with a concentration of 20 g / L, adjusting the pH value to 9, and then performing a neutralization reaction at 40° C. to obtain a neutralized product after 40 minutes; wherein the solvents of the aluminum nitrate solution and the aqueous ammonia solution are both methanol aqueous solution, and the mass ratio of methanol to water in the methanol aqueous solution is 6:1;

[0054] (2) subjecting the neutralized product obtained in step (1) to a crystallization reaction at 55° C. for 50 min, and then filtering to obtain a crystallized product;

[0055] (3) The crystallized product obtained in step (2) is mixed with water and (NH4)2CO3, and subjected to an aging reaction at 70°C for 80 minutes, and then filtered, and finally dried at 90°C for 60 minutes to obtain pseudo-boehmite; wherein the mass ratio of the crystallized product to (NH4)2CO3 is 20:1; and the pore volume of the pseudo-boehmite is 2.91 cm 3 / g, specific surface area is 552.6m 2 / g.

[0056] It can be seen from the above examples that the pseudo-boehmite prepared by the preparation method provided by the present invention has a high specific surface area and a large pore volume, and the pore volume can reach 2.91cm 3 / g, with a specific surface area of ​​up to 552.6m 2 / g.

[0057] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing pseudo-boehmite, comprising the following steps: (1) adding an aqueous ammonia solution to an aluminum nitrate solution, adjusting the pH value to 7 to 10, and performing a neutralization reaction to obtain a neutralized product; (2) subjecting the neutralized product obtained in step (1) to a crystallization reaction to obtain a crystallized product; (3) mixing the crystallized product obtained in step (2) with water and an auxiliary agent, and performing an aging reaction to obtain pseudo-boehmite; The concentration of the aluminum nitrate solution in step (1) is 20-30 g / L; the mass concentration of the ammonia solution is 2-3%; The temperature of the crystallization reaction in step (2) is 50-55° C., and the time of the crystallization reaction is 30-50 min; The temperature of the aging reaction in step (3) is 60-70° C., and the aging reaction time is 50-80 min; The auxiliary agent in step (3) includes one or more of (NH4)2CO3, NH4HCO3 and urea; the mass ratio of the crystallized product to the auxiliary agent is (15~20):

1.

2. The preparation method according to claim 1, characterized in that: In the step (1), the solvents of the aluminum nitrate solution and the ammonia solution are independently alcohol aqueous solutions.

3. The preparation method according to claim 2, characterized in that: The mass ratio of alcohol to water in the alcohol aqueous solution is (1-6):

1.

4. The preparation method according to claim 1, characterized in that: The temperature of the neutralization reaction in step (1) is 30-40° C., and the time of the neutralization reaction is 20-40 min.

5. Pseudo-boehmite prepared by the preparation method according to any one of claims 1 to 4.

6. The pseudo-boehmite according to claim 5, characterized in that: The pore volume of the pseudo-boehmite is 2.3-2.9 cm 3 / g, specific surface area is 500~550m 2 / g.

Citation Information

Cited By

  • Aperture-concentrated high-purity pseudo-boehmite and preparation method thereof

    CN122355323A

  • Pore size concentrated high-purity pseudo-boehmite and preparation method thereof

    CN122355323B