Glass for sealing sapphire and Kovar alloy and preparation method thereof

By using the new formula glass material to seal sapphire and coval alloy, the problems of short service life and high cost in high temperature environments in the prior art are solved, and the effects of high temperature resistance and cost reduction are achieved.

CN115974412BActive Publication Date: 2024-11-26BEIJING GLASS RES INST +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111194813.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-15
Publication Date
2024-11-26
Estimated Expiration
2041-10-15

AI Technical Summary

Technical Problem

The existing sapphire and covaler alloy sealing technology has a short service life and high cost in high temperature environments. The bonding method is aging and the welding method is high, which limits its application.

Method used

A new glass material formula, including silicon oxide, alumina, boron oxide, sodium oxide, strontium oxide, potassium oxide, calcium oxide, glass powder made by silicon molybdenum rod furnace and ball milling, is used for sapphire and The sealing of Korva alloy reduces cost and improves high temperature resistance.

Benefits of technology

It realizes the high temperature stability and reduces the sealing cost of sapphire and covaler alloy used in high temperature environments, and is suitable for mass production.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to the field of glass technology, and in particular to a sapphire and kovar alloy sealing glass and a preparation method thereof. The glass is prepared using the following raw material components: silicon oxide, aluminum oxide, boron oxide, sodium oxide, strontium oxide, potassium oxide, and calcium oxide. The sealing temperature of the sealing glass is 900-960°C, and the thermal expansion coefficient is 60-70×10 ‑7 / ℃, and the expansion softening point is 670‑695℃. Compared with the existing sapphire and Kovar alloy sealing methods, the use of sealing glass for sealing can effectively reduce the sealing cost, and the sealing glass has good high temperature resistance, so that the sealing product still has good stability in high temperature environment, providing a stable and reliable sealing material for sapphire and Kovar alloy sealing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of glass technology, and in particular to a glass for sealing sapphire and kovar alloy and a preparation method thereof. Background Art

[0002] At present, sapphire and Kovar alloy are usually sealed by gluing or welding. However, the sealing parts using gluing cannot be used in high temperature environments (above 300°C), and the sealant itself has aging phenomena, which seriously affects the service life of the sealing parts. Although the welding method can achieve a good sealing effect, the welding cost is high, which limits the application of this method to a certain extent. Sealing glass has the advantages of good insulation, high temperature resistance, and non-oxidation. It can be formulated according to the thermal expansion coefficient of different sealing parts. At the same time, sealing glass has good thermal stability and is widely used in sealing different types of materials, such as ceramics, metals and composite materials. Compared with brazing, the glass sealing method is cheaper and can be suitable for mass production.

[0003] The present invention studies and develops a high temperature resistant glass material for sealing Kovar alloy and sapphire, which can be used for sealing sapphire and Kovar alloy. Summary of the invention

[0004] The purpose of the present invention is to provide a glass for sealing sapphire and Kovar alloy and a preparation method thereof. The sealing material for sealing sapphire and Kovar alloy has good high temperature stability. While ensuring good sealing, it can reduce the sealing cost of sapphire and Kovar alloy.

[0005] The technical solution to the problem of the present invention is: a glass for sealing sapphire and Kovar alloy, comprising the following raw material components: silicon oxide SiO2, aluminum oxide Al2O3, boron oxide B2O3, sodium oxide Na2O, strontium oxide SrO, potassium oxide K2O, and calcium oxide CaO.

[0006] Furthermore, in the glass for sealing sapphire and kovar alloy of the present invention, the weight percentages of the raw material components of each sealing glass are as follows: silicon oxide is 40-60%, aluminum oxide is 5-10%, boron oxide is 10-15%, sodium oxide is 5-10%, strontium oxide is 6-15%, potassium oxide is 2-13%, and calcium oxide is 1-5%.

[0007] The present invention also provides a method for preparing the above-mentioned sapphire and kovar alloy sealing glass, which is characterized by comprising the following steps:

[0008] (1) According to the raw material components of the sapphire and kovar alloy sealing glass, silicon oxide, aluminum oxide, boron oxide, sodium oxide, strontium oxide, potassium oxide and calcium oxide are weighed and mixed thoroughly to prepare a mixture;

[0009] (2) adding the mixed material obtained in step (1) in batches into a corundum crucible in a silicon-molybdenum rod furnace at a feeding temperature of 1200-1350° C.;

[0010] (3) The temperature of the silicon-molybdenum rod furnace is set to 1400-1480°C, and the solution is stirred for the first time after heating for 2 hours, and stirred once every 1 hour, for a total of two times;

[0011] (4) After stirring, the mixed solution is melted at 1400-1480°C for 1-2h;

[0012] (5) taking the molten liquid from step (4) out of the furnace and quenching it with water to form glass slag;

[0013] (6) The glass slag obtained in step (5) is ball-milled to prepare glass powder, zirconium balls and glass are mixed in a weight ratio of 1:1, the amount of alcohol added is 500 ml / kg, and the particle size of the glass powder is 5-10 μm.

[0014] Preferably, in the method for preparing glass for sealing sapphire and kovar alloy of the present invention, in the step (4), the mixed solution is melted at 1460° C. for 1 hour.

[0015] Preferably, the sealing temperature of the glass for sealing sapphire and Kovar alloy of the present invention is 900-960°C.

[0016] Preferably, the thermal expansion coefficient of the glass for sealing sapphire and Kovar alloy of the present invention is 60-70×10 -7 / ℃.

[0017] Preferably, the expansion softening point of the glass for sealing sapphire and Kovar alloy of the present invention is 670-695°C.

[0018] Compared with the prior art, the present invention has the following beneficial effects: providing a glass for sealing sapphire and Kovar alloy, simplifying the sealing process of sapphire and Kovar alloy, reducing the sealing cost of sapphire and metal alloy, and improving the sealing efficiency. The sealed product has good high temperature resistance and is suitable for use in high temperature environment. DETAILED DESCRIPTION

[0019] The present invention is further described below with reference to specific embodiments, but the protection scope of the present invention is not limited thereto.

[0020] Unless otherwise specified, the experimental methods used in the following examples are conventional methods.

[0021] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.

[0022] Example 1

[0023] A glass for sealing sapphire and kovar alloy, the raw material components of which are 40% silicon oxide, 10% aluminum oxide, 15% boron oxide, 5% sodium oxide, 15% strontium oxide, 10% potassium oxide and 5% calcium oxide in weight percentage.

[0024] The method for preparing the above-mentioned sapphire and Kovar alloy sealing glass is as follows:

[0025] (1) fully mixing the raw materials of the sapphire and kovar alloy sealing glass to prepare a mixed material;

[0026] (2) adding the mixed material obtained in step (1) in batches into a corundum crucible in a silicon-molybdenum rod furnace at a feeding temperature of 1200° C.;

[0027] (3) The temperature of the silicon-molybdenum rod furnace was set to 1400°C. After heating for 2 hours, the solution was stirred for the first time, and then stirred once every 1 hour for a total of two times.

[0028] (4) After stirring, the mixed solution was melted at 1400°C for 2 h.

[0029] (5) The molten liquid in step (4) is taken out of the furnace and water quenched to form glass slag.

[0030] (6) The glass slag obtained in step (5) is ball-milled to prepare glass powder, zirconium balls and glass are mixed in a weight ratio of 1:1, the amount of alcohol added is 500 ml / kg, and the particle size of the glass powder is 5-10 μm.

[0031] The basic performance test of the sealing glass of the present invention is carried out by the following method:

[0032] (1) Sealing temperature test: Use a high temperature physical property tester to measure the wetting angle and high temperature physical properties of the glass to determine the sealing temperature of the glass;

[0033] (2) Thermal expansion coefficient test: Use an expansion coefficient tester to measure the thermal expansion coefficient of glass;

[0034] (3) Softening point test: Use an expansion coefficient tester to measure the expansion softening point of the glass;

[0035] The specific performance test results are shown in Table 1. The sealing temperature is 900-920℃, and the thermal expansion coefficient is 70×10 -7 / ℃, expansion softening point is 670℃.

[0036] Example 2

[0037] A glass for sealing sapphire and Kovar alloy, the raw material components of which are 45% silicon oxide, 12% aluminum oxide, 10% boron oxide, 6% sodium oxide, 12% strontium oxide, 13% potassium oxide and 2% calcium oxide in weight percentage.

[0038] The method for preparing the above-mentioned sapphire and Kovar alloy sealing glass is as follows:

[0039] (1) fully mixing the raw materials of the sapphire and kovar alloy sealing glass to prepare a mixed material;

[0040] (2) adding the mixed material obtained in step (1) in batches into a corundum crucible in a silicon-molybdenum rod furnace at a feeding temperature of 1250° C.;

[0041] (3) The temperature of the silicon-molybdenum rod furnace was set to 1420°C. After heating for 2 hours, the solution was stirred for the first time, and then stirred once every 1 hour for a total of two times.

[0042] (4) After stirring, the mixed solution was melted at 1420°C for 2 h.

[0043] (5) The molten liquid in step (4) is taken out of the furnace and water quenched to form glass slag.

[0044] (6) The glass slag obtained in step (5) is ball-milled to prepare glass powder, zirconium balls and glass are mixed in a weight ratio of 1:1, the amount of alcohol added is 500 ml / kg, and the particle size of the glass powder is 5-10 μm.

[0045] The specific performance test results are shown in Table 1. The sealing temperature is 900-920℃, and the thermal expansion coefficient is 65×10 -7 / ℃, expansion softening point is 674℃.

[0046] Example 3

[0047] A glass for sealing sapphire and kovar alloy, the raw material components of which are 50% silicon oxide, 8% aluminum oxide, 12% boron oxide, 10% sodium oxide, 10% strontium oxide, 8% potassium oxide and 1% calcium oxide in weight percentage.

[0048] The method for preparing the above-mentioned sapphire and Kovar alloy sealing glass is as follows:

[0049] (1) fully mixing the raw materials of the sapphire and kovar alloy sealing glass to prepare a mixed material;

[0050] (2) adding the mixed material obtained in step (1) in batches into a corundum crucible in a silicon-molybdenum rod furnace at a feeding temperature of 1280° C.;

[0051] (3) The temperature of the silicon-molybdenum rod furnace was set to 1450°C. After heating for 2 hours, the solution was stirred for the first time, and then stirred once every 1 hour for a total of two times.

[0052] (4) After stirring, the mixed solution was melted at 1450°C for 2 h.

[0053] (5) The molten liquid in step (4) is taken out of the furnace and water quenched to form glass slag.

[0054] (6) The glass slag obtained in step (5) is ball-milled to prepare glass powder, zirconium balls and glass are mixed in a weight ratio of 1:1, the amount of alcohol added is 500 ml / kg, and the particle size of the glass powder is 5-10 μm.

[0055] The specific performance test results are shown in Table 1. The sealing temperature is 910-940℃, and the thermal expansion coefficient is 64×10 -7 / ℃, expansion softening point is 680℃.

[0056] Example 4

[0057] A glass for sealing sapphire and Kovar alloy, the raw material components of which are 55% silicon oxide, 6% aluminum oxide, 15% boron oxide, 9% sodium oxide, 8% strontium oxide, 2% potassium oxide and 5% calcium oxide in weight percentage.

[0058] The method for preparing the above-mentioned sapphire and Kovar alloy sealing glass is as follows:

[0059] (1) fully mixing the raw materials of the sapphire and kovar alloy sealing glass to prepare a mixed material;

[0060] (2) adding the mixed material obtained in step (1) in batches into a corundum crucible in a silicon-molybdenum rod furnace at a feeding temperature of 1300° C.;

[0061] (3) The temperature of the silicon-molybdenum rod furnace was set to 1460°C. After heating for 2 hours, the solution was stirred for the first time, and then stirred once every 1 hour for a total of two times.

[0062] (4) After stirring, the mixed solution was melted at 1460°C for 1 h.

[0063] (5) The molten liquid in step (4) is taken out of the furnace and water quenched to form glass slag.

[0064] (6) The glass slag obtained in step (5) is ball-milled to prepare glass powder, zirconium balls and glass are mixed in a weight ratio of 1:1, the amount of alcohol added is 500 ml / kg, and the particle size of the glass powder is 5-10 μm.

[0065] The specific performance test results are shown in Table 1. The sealing temperature is 920-950℃, and the thermal expansion coefficient is 62×10 -7 / ℃, the expansion softening point is 687℃.

[0066] Example 5

[0067] A glass for sealing sapphire and Kovar alloy, the raw material components of which are 60% silicon oxide, 5% aluminum oxide, 10% boron oxide, 8% sodium oxide, 6% strontium oxide, 7% potassium oxide and 4% calcium oxide in weight percentage.

[0068] The method for preparing the above-mentioned sapphire and Kovar alloy sealing glass is as follows:

[0069] (1) fully mixing the raw materials of the sapphire and kovar alloy sealing glass to prepare a mixed material;

[0070] (2) adding the mixed material obtained in step (1) in batches into a corundum crucible in a silicon-molybdenum rod furnace at a feeding temperature of 1350° C.;

[0071] (3) The temperature of the silicon-molybdenum rod furnace was set to 1480°C. After heating for 2 hours, the solution was stirred for the first time, and then stirred once every 1 hour for a total of two times.

[0072] (4) After stirring, the mixed solution was melted at 1480°C for 1 h.

[0073] (5) The molten liquid in step (4) is taken out of the furnace and water quenched to form glass slag.

[0074] (6) The glass slag obtained in step (5) is ball-milled to prepare glass powder, zirconium balls and glass are mixed in a weight ratio of 1:1, the amount of alcohol added is 500 ml / kg, and the particle size of the glass powder is 5-10 μm.

[0075] The specific performance test results are shown in Table 1. The sealing temperature is 940-960℃, and the thermal expansion coefficient is 60×10 -7 / ℃, expansion softening point is 695℃.

[0076] Table 1 Performance test table

[0077] Glass properties Example 1 Example 2 Example 3 Example 4 Example 5 Sealing temperature(℃) 900-920 900-920 910-940 920-950 940-960 <![CDATA[Coefficient of thermal expansion (×10 -7 / °C)]]> 70 65 64 62 60 <![CDATA[Swelling softening point T f (°C)]]> 670 674 680 687 695

[0078] The present invention is not limited to the above-mentioned embodiments. Without departing from the essential content of the present invention, any deformation, improvement and substitution that can be conceived by those skilled in the art shall fall within the scope of the present invention.

Claims

1. A method for preparing glass for sealing sapphire and Kovar alloy, characterized in that: The glass for sealing sapphire and Kovar alloy is composed of the following raw material components: silicon oxide, aluminum oxide, boron oxide, sodium oxide, strontium oxide, potassium oxide, and calcium oxide, wherein the weight percentages of the raw material components are as follows: silicon oxide is 40-60%, aluminum oxide is 5-10%, boron oxide is 10-15%, sodium oxide is 5-10%, strontium oxide is 8-15%, potassium oxide is 2-13%, and calcium oxide is 1-5%; The preparation method of glass for sealing sapphire and Kovar alloy comprises the following steps: (1) According to the raw material components of the glass for sealing sapphire and Kovar alloy, silicon oxide, aluminum oxide, boron oxide, sodium oxide, strontium oxide, potassium oxide, and calcium oxide are weighed and fully mixed to prepare a mixture; (2) adding the mixed material obtained in step (1) in batches into a corundum crucible in a silicon-molybdenum rod furnace at a feeding temperature of 1200-1350° C.; (3) The temperature of the silicon-molybdenum rod furnace is set to 1400-1480°C, and the solution is stirred for the first time after heating for 2 hours, and stirred once every 1 hour, for a total of two times; (4) After stirring, the mixed solution is melted at 1400-1480°C for 1-2h; (5) taking the molten liquid from step (4) out of the furnace and quenching it with water to form glass slag; (6) The glass slag obtained in step (5) is ball-milled to form glass powder, the zirconium balls and the glass slag are mixed in a weight ratio of 1:1, the alcohol addition amount is 500 ml / kg, and the particle size of the glass powder is 5-10 μm.

2. The method for preparing glass for sealing sapphire and kovar alloy according to claim 1, characterized in that: The sealing temperature of the glass used for sealing the sapphire and the Kovar alloy is 900-960°C.

3. The method for preparing the glass for sealing sapphire and kovar alloy according to claim 1 or 2, characterized in that: The thermal expansion coefficient of the glass used for sealing sapphire and Kovar alloy is 60-70×10 -7 / ℃.

4. The method for preparing glass for sealing sapphire and kovar alloy according to claim 1 or 2, characterized in that: The expansion softening point of the glass used for sealing the sapphire and Kovar alloy is 670-695°C.

5. The method for preparing glass for sealing sapphire and kovar alloy according to claim 1, characterized in that: In the step (4), the mixed solution is melted at 1460° C. for 1 hour.