A composite photothermal fabric with high evaporation performance and preparation method thereof
By preparing composite photothermal fabrics, combining carbon-based polymer porous membranes and hydrophilic fabrics, the problems of complex preparation, high cost, and insufficient durability of existing photo-steam conversion materials have been solved, achieving high efficiency in photo-steam conversion and water evaporation performance, which is suitable for seawater desalination and wastewater treatment.
Patent Information
- Application Number
- CN202310011280.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-05
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-01-05
AI Technical Summary
Existing photo-steam conversion materials suffer from problems such as complex preparation, high cost, poor performance, and insufficient durability in seawater desalination and wastewater treatment, making it difficult to meet practical application needs.
A composite photothermal fabric structure, consisting of a carbon-based polymer porous membrane and a hydrophilic fabric, is prepared by a water droplet template method to form a hierarchical porous structure. This structure combines carbon-based nanoparticles and polymers to improve light absorption and water vapor dissipation capabilities, thereby enhancing mechanical properties.
It achieves high photo-steam conversion efficiency and water evaporation rate, improves the durability and recyclability of materials, reduces preparation costs, and is suitable for seawater desalination and wastewater treatment.
Smart Images

Figure CN115976851B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of environmental energy application, and relates to a composite photothermal fabric with high evaporation performance and a preparation method thereof. Background Art
[0002] Today's social and economic development faces two major challenges: the shortage of fresh water resources and the crisis of traditional fossil energy. The desalination and wastewater treatment based on solar steam generation technology absorbs solar energy and converts it into thermal energy through photothermal materials, heats seawater or wastewater to generate water vapor, and condenses it to achieve fresh water recovery. This technology is of great significance because it uses clean and pollution-free energy and is inexhaustible. In recent years, interfacial photo-steam conversion technology has achieved more efficient photo-steam conversion by localizing heat on the surface of water.
[0003] Studies have shown that the porous structure of the surface of interfacial light-steam conversion materials is conducive to the escape of water vapor, which can ensure efficient light-steam conversion and thus achieve sufficient fresh water recovery.
[0004] Chinese patent CN 111285704 A obtains cellulose-based carbon-based photothermal conversion materials for seawater desalination by carbonizing cellulose-based porous materials prepared by freeze-drying nanocellulose. Its rich and porous network structure can provide a channel for the escape of water vapor during the photothermal conversion process. However, the preparation method of this interface photothermal conversion material is complicated, costly, and has poor performance (when treating simulated seawater, its maximum water evaporation rate can only reach 1.211 kg m -2 h -1 The maximum light-to-steam conversion efficiency can only reach 84.78%, which makes practical application difficult.
[0005] Chinese patent CN 112898954 A freeze-dries the cut Pleurotus eryngii, and then places it in a photothermal conversion material modification reaction liquid, so that the photothermal conversion material is adsorbed on the porous structure and surface of the Pleurotus eryngii, and finally freeze-dried to obtain the Pleurotus eryngii-based photothermal conversion material. The porous structure inside the material itself ensures the transmission of water and the escape of surface water vapor, and has the advantages of high water evaporation rate, low cost, and environmental friendliness. However, since the material is carbonized Pleurotus eryngii, it does not have good mechanical properties, so it is difficult to meet the processing requirements under actual conditions.
[0006] It can be seen that while ensuring the escape of water vapor and efficient photo-steam conversion, the durability of the photo-steam conversion material cannot be ignored, which is crucial for the practical application of the material in seawater desalination and wastewater treatment. Summary of the invention
[0007] The purpose of the present invention is to solve the above problems existing in the prior art and to provide a composite photothermal fabric with high evaporation performance and a preparation method thereof.
[0008] To achieve the above object, the technical solution adopted by the present invention is as follows:
[0009] A composite photothermal fabric with high evaporation performance, comprising a photothermal layer and a base layer adjacent thereto;
[0010] The photothermal layer is a carbon-based polymer porous membrane, mainly composed of polymers and carbon-based nanoparticles dispersed therein; the thickness of the photothermal layer is 10 to 100 μm, the average pore size is 1 to 10 μm, and the porosity is 65% to 95%; the appropriate pore size of the photothermal layer is not only conducive to increasing the optical traps on the surface of the photothermal layer, extending the optical path, and achieving maximum capture and absorption of light, but also can provide a channel for the escape of water vapor during the photo-steam conversion process; the appropriate thickness of the photothermal layer is conducive to achieving maximum light absorption, excessive thickness causes a decrease in internal permeability, thereby affecting the escape of steam, while too small thickness has a short optical path, which is not conducive to effective absorption of light; in addition, generally speaking, the higher the porosity, the better the internal permeability, the more sufficient the absorption of light and the escape of steam, which is conducive to achieving greater light absorption;
[0011] The polymer is a hydrophilic polymer or a hydrophobic polymer; when the polymer is a hydrophilic polymer, the photothermal layer can be hydrophilic to accelerate the reflux of salt ions; when the polymer is a hydrophobic polymer, the photothermal layer can be hydrophobic to resist salt crystallization, because the surface hydrophobicity hinders the transport of the aqueous solution containing salt ions, thereby effectively hindering the deposition of salt;
[0012] The base layer is a hydrophilic fabric.
[0013] The function of the upper photothermal layer in the present invention is to increase light absorption, vapor dissipation, hydrophobic and salt-repelling (hydrophilic and salt-repelling), and the carbon-based nanoparticles provide photothermal conversion. The function of the lower base layer is hydrophilic and conducive to water transportation. In addition, the flexible material is also convenient for transportation and storage. The mechanical effect of the fabric is good, which is conducive to improving the durability of the product.
[0014] The present invention has good light absorption performance, excellent water vapor dissipation ability and efficient water transport performance, which can ensure efficient water evaporation. In addition, the materials used in the present invention are flexible fabrics and plastic polymers with excellent mechanical properties, so excellent mechanical and wearing properties can be achieved to meet actual needs.
[0015] As the preferred technical solution:
[0016] The composite photothermal fabric with high evaporation performance has a light absorption rate of more than 90% and an air permeability of 201 to 291 mm·s -1 , moisture permeability is 2983~3392g·m-2 ·d -1 ;
[0017] The photothermal conversion efficiency of the composite photothermal fabric to pure water is 85.2% to 98.2%, and the water evaporation rate is 1.12 to 1.41 kg·m -2 ·h -1 ;
[0018] The photothermal conversion efficiency of the composite photothermal fabric for 3.5wt% NaCl aqueous solution is 81.4% to 92.1%, and the water evaporation rate is 1.01 to 1.37 kg·m -2 ·h -1 ;
[0019] The composite photothermal fabric can be recycled for no less than 15 times.
[0020] The photo-steam conversion efficiency of the composite photo-thermal fabric of the present invention (the photo-steam conversion efficiency for 3.5wt% NaCl aqueous solution is 81.4% to 92.1%) is better than that of the currently disclosed photo-thermal fabrics. For example, the photo-steam conversion efficiency of the three-dimensional porous seawater desalination thermal evaporation material disclosed in the prior art, CN111074534B, for seawater is greater than 80%. The patent CN111074534B only briefly mentions that the photo-steam conversion efficiency of the seawater of the material is greater than 80% in the claims. In the subsequent description and its embodiments, there is no specific data clearly indicating the photo-steam conversion efficiency of the seawater of the material. Actual tests show that the photo-steam conversion efficiency of the material for seawater is only about 80%. For example, the photo-steam conversion efficiency of the carbon black / cellulose composite photo-thermal material disclosed in CN111285704A for seawater does not exceed 84.78%. For example, the photo-steam conversion efficiency of the full-fiber three-dimensional aggregate disclosed in CN111645244A for simulated seawater is only 86.5%;
[0021] The durability (recyclability of not less than 15 times) of the composite photothermal fabric of the present invention is superior to the currently disclosed photothermal fabrics. Most of the photothermal fabrics involved in the prior art, such as patent CN111074534B, patent CN113882154A, patent CN112980399A and patent CN111348708B, are obtained by impregnation, deposition and loading treatment. It is difficult for the photothermal particles to achieve good bonding with the fabric, resulting in poor recycling practicality of the photothermal fabric. The photothermal particles (carbon-based nanoparticles) of the present invention are mixed with polymers to form a porous film through a water drop template method. The photothermal particles are coated in the polymer and are difficult to fall off. In addition, the halogen elements in the polymer are easy to combine with the -OH bonds in the fabric to form a stable chemical bond, thereby greatly improving the recycling of the photothermal fabric.
[0022] As described above, in a composite photothermal fabric with high evaporation performance, the average pore size of the base layer is larger than the average pore size of the photothermal layer; when the base layer and the photothermal layer are both porous structures and the average pore size of the base layer is larger than the average pore size of the photothermal layer, a differential capillary effect is formed due to the difference in wicking pressure gradients from large pore size to small pore size between the upper and lower layers, thereby realizing directional water transport from the water body to the base layer and then to the photothermal layer.
[0023] As described above, a composite photothermal fabric with high evaporation performance has a base layer thickness of 400-600 μm, an average pore size of 10-50 μm, and a porosity of 80%-99%. Compared with the photothermal layer, the thicker base layer and sufficient porosity are conducive to the storage of water therein for easy photoevaporation, and the larger pore size facilitates the formation of a capillary differential effect with the small pore size of the photothermal layer, thereby realizing directional transport of water.
[0024] As described above, a composite photothermal fabric with high evaporation performance, the carbon-based nanoparticles are one or more of carbon black, graphene oxide, redox graphene and carbon nanotubes; the carbon-based nanoparticles are naturally black and suitable for broadband solar energy absorption. The absorption of solar energy by the carbon-based nanoparticles includes the excitation of electrons and their subsequent relaxation phenomena. The scattering between electrons and electrons and electrons and phonons causes the photoexcited electrons to thermalize rapidly to generate heat energy. The cost is low and the processability is good.
[0025] As described above, the composite photothermal fabric with high evaporation performance, the polymer is one or more of polypropylene butadiene copolymer, polydimethylsiloxane, polystyrene, polysulfone resin, polyphenylene ether sulfone, polyetherimide, cellulose acetate, methyl cellulose, carboxymethyl cellulose, ethyl cellulose, hydroxyethyl cellulose, cyanoethyl cellulose, hydroxypropyl cellulose and hydroxypropyl methyl cellulose.
[0026] As described above, the composite photothermal fabric with high evaporation performance, the hydrophilic fabric is cotton fabric, spandex fabric, viscose fiber fabric, modal fiber fabric, lyocell fiber fabric, bamboo fiber fabric, wool fabric, hydrophilized polyester fabric, hydrophilized acrylic fabric, hydrophilized nylon fabric, hydrophilized aramid fabric or hydrophilized carbon fiber fabric, and the hydrophilization treatment can be carried out by graft copolymerization or by blending and compounding with hydrophilic substances.
[0027] As described above, in a composite photothermal fabric with high evaporation performance, the polymer is polypropylene butadiene copolymer, and the hydrophilic fabric is cotton fabric; or, the polymer is polystyrene, and the hydrophilic fabric is cotton fabric; or, the polymer is cellulose acetate, and the hydrophilic fabric is modal fiber fabric; or, the polymer is polyphenylene ether sulfone, and the hydrophilic fabric is lyocell fiber fabric; or, the polymer is hydroxypropyl cellulose, and the hydrophilic fabric is hydrophilized aramid fabric; such selection of polymer and hydrophilic fabric allows the two to be chemically bonded during the preparation process, thereby enhancing the bonding force between the photothermal layer and the base layer, which is beneficial to improving the recyclability of the product.
[0028] The present invention also provides a method for preparing a composite photothermal fabric with high evaporation performance as described in any of the above items, after coating the carbon-based nanoparticle / polymer mixed solution on the hydrophilic fabric, forming the carbon-based polymer porous membrane by a water drop template method, thereby obtaining a composite photothermal fabric with high evaporation performance, wherein the carbon-based nanoparticle / polymer mixed solution is mainly composed of the carbon-based nanoparticles, the polymer and a solvent; the solvent is acetone, chloroform, dimethylformamide, toluene and ethylene glycol, etc.
[0029] Since the photothermal layer prepared by the water droplet template method has a hierarchical porous structure, the present invention has certain advantages in two important performance indicators of photothermal fabrics: light absorption rate (holes are beneficial to extend the path of light and reduce light reflection) and light-to-steam conversion efficiency (porous structure can reduce the loss of light energy and increase the escape of water vapor).
[0030] As the preferred technical solution:
[0031] According to the method described above, the preparation process of the carbon-based nanoparticle / polymer mixed solution is as follows:
[0032] (1) adding the polymer to the solvent, stirring at a speed of 1000 to 5000 r / min at 30 to 50° C. for 1 to 5 hours, to obtain a polymer solution; the concentration of the polymer in the polymer solution is 50 to 300 g / L;
[0033] (2) Adding carbon-based nanoparticles to the polymer solution, stirring for 1 to 6 hours, and then ultrasonicating for 10 to 60 minutes to obtain a carbon-based nanoparticle / polymer mixed solution; the concentration of the carbon-based nanoparticles in the carbon-based nanoparticle / polymer mixed solution is 5 to 50 g / L.
[0034] The method as described above has the following specific process: the hydrophilic fabric is ironed and finished, and a carbon-based nanoparticle / polymer mixed solution is coated on its surface with a scraper (the thickness of the mixed solution on the fabric surface should be ensured to be uniform and flat), and then it is quickly placed in a closed environment with a temperature of 20 to 60°C and a relative humidity of 65% to 99% and left to stand for 0.5 to 5 hours to obtain a composite photothermal fabric with high evaporation performance.
[0035] The principle of the present invention is as follows:
[0036] The mechanism of pore formation of composite photothermal fabric in high humidity environment is mainly as follows: the mixed solution coated on the surface of the fabric has a volatile solvent, which will cause the surface temperature of the carbon-based layer to drop during the volatilization process, so that the water vapor in the high humidity environment condenses into water droplets on the surface of the mixed solution, and assembles into a water drop array with a closed arrangement structure under various conditions. When the composite photothermal fabric leaves the high humidity environment, due to the evaporation of the surface water droplets, a honeycomb porous ordered structure is formed on the surface of the polymer layer of the fabric. In this process, the size of the polymer molecules, the volatility of the solvent, the concentration of the polymer, and the different environments will affect the pore formation on the surface of the carbon-based composite fabric. The present invention can prepare a composite photothermal fabric with a certain size, uniform distribution and through pores by adjusting various factors.
[0037] Beneficial Effects
[0038] (1) The composite photothermal fabric prepared by the present invention has excellent air permeability and moisture permeability. Compared with other materials or surface-sealed interface photothermal conversion materials, the pore size on the surface of the composite photothermal fabric can provide an escape channel for water vapor generated during the photothermal conversion process, which can firstly increase the photothermal conversion efficiency and secondly facilitate the subsequent condensation and recovery of water vapor;
[0039] (2) The composite photothermal fabric prepared by the present invention has excellent light absorption capacity. The carbon-based nanoparticles themselves have high light absorption and good photothermal conversion effect, and can convert the absorbed light energy into thermal energy. In addition, the aperture of the composite photothermal fabric can increase optical traps, extend the optical path, increase the refraction and reflection of light on the surface, increase the light capture ability, and achieve the maximum light absorption effect;
[0040] (3) The preparation method of the present invention is simple and the material cost is low;
[0041] (4) The water drop template method used in the present invention can achieve effective regulation of the pore size and hydrophilic and hydrophobic properties of the composite photothermal fabric surface by changing the materials and process parameters, and has strong designability;
[0042] (5) The preparation method of the present invention achieves the regulation of the hydrophilicity and hydrophobicity of the photothermal layer by selecting polymer materials, thereby realizing the multifunctionality of the composite photothermal fabric in practical applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 This is the preparation process of the composite photothermal fabric of Example 4 of the present invention;
[0044] Figure 2 This is a microstructure diagram of a composite photothermal fabric prepared in Example 4 of the present invention, wherein Figure a is a side view of the composite photothermal fabric, Figure b is a side view of the carbon-based polymer porous membrane, Figure c is a front view of the fabric, Figure d is a surface microstructure diagram of the carbon-based polymer porous membrane, and Figures e and f are partial enlarged schematic diagrams of Figure d. DETAILED DESCRIPTION
[0045] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0046] Method for testing relevant properties of the composite photothermal fabric with high evaporation performance prepared in the embodiment:
[0047] The light absorption rate detection method of the composite photothermal fabric is as follows: the light absorption capacity of the material sample within the spectral range of 250-2500nm is tested by using an ultraviolet spectrophotometer of model Hitachi UV3600;
[0048] Testing method for air permeability of composite photothermal fabric: Fully automatic air permeability tester (YG461H) is used for air permeability testing, with a test pressure of 200Pa and a test area of 20cm 2 , each sample was tested 5 times, and the average value was taken as the air permeability of the sample;
[0049] Testing method for moisture permeability of composite photothermal fabric: using a moisture permeability meter (model YG601H) and referring to standard GB / T12704.1 for testing; the sample is 70mm 2 The temperature of the moisture permeability chamber is 38℃, the relative humidity is 90%, and the air flow velocity is 0.5m / s. Each sample is tested at least 5 times and the average value is taken.
[0050] The test method for the evaporation rate of pure water is as follows: a material sample of 2×2 cm is floated on the water surface in a beaker through foam (foam wrapped in non-woven fabric with excellent hygroscopicity), and the beaker is placed on an electronic balance under the light source. The electronic balance is connected to a computer and records the evaporation rate of a solar light intensity (1kW / m 2) in the beaker within 60 minutes, and then calculate the mass loss of pure water per unit area of the material sample in kg m -2 Turn off the light source and record the mass loss of pure water per unit area of the material sample in the dark field environment within 60 minutes in the same way (in kg m -2 Finally, the evaporation rate of pure water is calculated based on the difference in mass loss of pure water in the bright field and dark field of the material sample per unit time, and the unit is kg m -2 h -1 ;
[0051] Testing method for the light vapor conversion efficiency of pure water: During the test of the water evaporation rate of pure water, under light conditions, a thermocouple is used to record the change of the surface temperature of the material over time, and the light vapor conversion efficiency η is calculated according to the following formula:
[0052]
[0053] ΔH=ΔH water +ΔH vapor ;
[0054] Where m is the steam flux, in kg·m -2 ·h -1 ; ΔH is the total enthalpy of liquid vapor phase change, including the sensible enthalpy change of water ΔH water and latent heat of phase change ΔH vapor (Unit: J / g); A is the area of the fabric sample receiving solar illumination; q Solar is the intensity of sunlight;
[0055] The detection method of the light-to-steam conversion efficiency of NaCl aqueous solution is basically the same as the above-mentioned light-to-steam conversion efficiency test of pure water, except that the NaCl aqueous solution is used in the detection process;
[0056] The test method for the water evaporation rate of NaCl aqueous solution is basically the same as the test method for the water evaporation rate of pure water, except that the NaCl aqueous solution is used in the test process;
[0057] Testing method for the number of cycles of composite photothermal fabrics: After conducting the above-mentioned water evaporation rate or light vapor conversion efficiency test, take out the material sample, clean it, let it stand and dry it, and then continue the same test for the next time until the sample surface is damaged or the test result has a significant decrease, and record the number of cycle tests of the material sample.
[0058] Example 1
[0059] A method for producing a composite photothermal fabric with high evaporation performance, the specific steps are as follows:
[0060] (1) Prepare raw materials:
[0061] Carbon-based nanoparticles: carbon nanotubes (manufacturer: Shanghai Baiyan Industrial Co., Ltd., brand name: C311);
[0062] Polymer: polydimethylsiloxane (manufacturer: Aladdin Chemical Reagent Co., Ltd., brand number: P195721-50g);
[0063] Hydrophilic fabric: Hydrophilic treated carbon fiber fabric (manufacturer: Shanghai Zhongcai Cotton Textile Co., Ltd., weight: 50g / m 2 );
[0064] Solvent: acetone (manufacturer: Aladdin Chemical Reagent Co., Ltd.);
[0065] (2) Preparation of carbon-based nanoparticle / polymer mixed solution:
[0066] (2.1) Add the polymer to the solvent and stir at 40°C for 5 h at a speed of 1000 r / min to obtain a polymer solution; the concentration of the polymer in the polymer solution is 50 g / L;
[0067] (2.2) adding carbon-based nanoparticles to the polymer solution, stirring for 2 h, and then ultrasonicating for 20 min to obtain a carbon-based nanoparticle / polymer mixed solution; the concentration of the carbon-based nanoparticles in the carbon-based nanoparticle / polymer mixed solution is 5 g / L;
[0068] (3) Preparation of composite photothermal fabrics:
[0069] The hydrophilic fabric was ironed and coated with a carbon-based nanoparticle / polymer mixed solution using a scraper, and then quickly placed in a closed environment with a temperature of 20°C and a relative humidity of 70% for 5 hours (water droplet template method) to obtain a composite photothermal fabric with high evaporation performance.
[0070] A composite photothermal fabric with high evaporation performance prepared by the above method is composed of a carbon-based polymer porous membrane and a hydrophilic fabric. The carbon-based polymer porous membrane is mainly composed of a polymer and carbon-based nanoparticles dispersed therein; the carbon-based polymer porous membrane has a thickness of 15 μm, an average pore size of 10 μm, and a porosity of 95%; the hydrophilic fabric has a thickness of 400 μm, an average pore size of 20 μm, and a porosity of 86%;
[0071] The light absorption rate of the composite photothermal fabric is 90%, and the air permeability is 291mm·s -1 , moisture permeability is 3392g·m -2 ·d -1 The light vapor conversion efficiency of pure water is 86.7%, and the water evaporation rate is 1.16 kg·m -2 ·h -1The light vapor conversion efficiency of 3.5wt% NaCl aqueous solution is 83.1%, and the water evaporation rate is 1.08kg·m -2 ·h -1 ; The composite photothermal fabric can be recycled 15 times.
[0072] Example 2
[0073] A method for producing a composite photothermal fabric with high evaporation performance, the specific steps are as follows:
[0074] (1) Prepare raw materials:
[0075] Carbon-based nanoparticles: graphene oxide (manufacturer: Qinghe County Tenghui Metal Materials Co., Ltd., brand number 10012);
[0076] Polymer: polyetherimide (manufacturer: Roen Chemical Reagent Co., Ltd., brand number: 700207-250g);
[0077] Hydrophilic fabric: Nylon fabric that has been hydrophilized (manufacturer: Tongxiang Allegans Textile Co., Ltd., weight 45g / m 2 );
[0078] Solvent: ethylene glycol (manufacturer: Roen Chemical Reagent Co., Ltd.);
[0079] (2) Preparation of carbon-based nanoparticle / polymer mixed solution:
[0080] (2.1) Add the polymer to the solvent and stir at 50°C for 3 h at a speed of 3000 r / min to obtain a polymer solution; the concentration of the polymer in the polymer solution is 70 g / L;
[0081] (2.2) adding carbon-based nanoparticles to the polymer solution, stirring for 3 h, and then ultrasonicating for 10 min to obtain a carbon-based nanoparticle / polymer mixed solution; the concentration of the carbon-based nanoparticles in the carbon-based nanoparticle / polymer mixed solution is 10 g / L;
[0082] (3) Preparation of composite photothermal fabrics:
[0083] The hydrophilic fabric was ironed and coated with a carbon-based nanoparticle / polymer mixed solution using a scraper, and then quickly placed in a closed environment with a temperature of 20°C and a relative humidity of 65% for 2 hours (water droplet template method) to obtain a composite photothermal fabric with high evaporation performance.
[0084] A composite photothermal fabric with high evaporation performance prepared by the above method is composed of a carbon-based polymer porous membrane and a hydrophilic fabric. The carbon-based polymer porous membrane is mainly composed of a polymer and carbon-based nanoparticles dispersed therein; the carbon-based polymer porous membrane has a thickness of 20 μm, an average pore size of 9 μm, and a porosity of 95%; the hydrophilic fabric has a thickness of 400 μm, an average pore size of 40 μm, and a porosity of 92%;
[0085] The light absorption rate of the composite photothermal fabric is 92.3% and the air permeability is 283mm·s -1 , moisture permeability is 3304g·m -2 ·d -1 The light vapor conversion efficiency of pure water is 98.2%, and the water evaporation rate is 1.37 kg·m -2 ·h -1 The light vapor conversion efficiency of 3.5wt% NaCl aqueous solution is 92.1%, and the water evaporation rate is 1.21kg·m -2 ·h -1 ; The composite photothermal fabric can be recycled 15 times.
[0086] Example 3
[0087] A method for producing a composite photothermal fabric with high evaporation performance, the specific steps are as follows:
[0088] (1) Prepare raw materials:
[0089] Carbon-based nanoparticles: redox graphene (manufacturer: Qinghe County Tenghui Metal Materials Co., Ltd., brand name: XF248-7440-44-0);
[0090] Polymer: polyphenylene ether sulfone (manufacturer: Shanghai Boer Chemical Reagent Co., Ltd., brand number: CB5945326);
[0091] Hydrophilic fabric: bamboo fiber fabric (manufacturer: Jiangsu Carnation Weaving Co., Ltd., weight 50g / m 2 );
[0092] Solvent: dimethylformamide (manufacturer: Shanghai Boer Chemical Reagent Co., Ltd.);
[0093] (2) Preparation of carbon-based nanoparticle / polymer mixed solution:
[0094] (2.1) Add the polymer to the solvent and stir at 35°C for 2 h at a speed of 2500 r / min to obtain a polymer solution; the concentration of the polymer in the polymer solution is 100 g / L;
[0095] (2.2) adding carbon-based nanoparticles to the polymer solution, stirring for 1 hour, and then ultrasonicating for 30 minutes to obtain a carbon-based nanoparticle / polymer mixed solution; the concentration of the carbon-based nanoparticles in the carbon-based nanoparticle / polymer mixed solution is 20 g / L;
[0096] (3) Preparation of composite photothermal fabrics:
[0097] The hydrophilic fabric was ironed and coated with a carbon-based nanoparticle / polymer mixed solution using a scraper, and then quickly placed in a closed environment with a temperature of 40°C and a relative humidity of 78% for 3 hours (water droplet template method) to obtain a composite photothermal fabric with high evaporation performance.
[0098] A composite photothermal fabric with high evaporation performance prepared by the above method is composed of a carbon-based polymer porous membrane and a hydrophilic fabric. The carbon-based polymer porous membrane is mainly composed of a polymer and carbon-based nanoparticles dispersed therein; the carbon-based polymer porous membrane has a thickness of 30 μm, an average pore size of 7.5 μm, and a porosity of 94%; the hydrophilic fabric has a thickness of 430 μm, an average pore size of 50 μm, and a porosity of 99%;
[0099] The light absorption rate of the composite photothermal fabric is 93.1% and the air permeability is 274mm·s -1 , moisture permeability is 3265g·m -2 ·d -1 The photo-vapor conversion efficiency of pure water is 96.4%, and the water evaporation rate is 1.41 kg·m -2 ·h -1 The light vapor conversion efficiency of 3.5wt% NaCl aqueous solution is 90.1%, and the water evaporation rate is 1.37kg·m -2 ·h -1 ; The composite photothermal fabric can be recycled 15 times.
[0100] Example 4
[0101] A method for composite photothermal fabrics with high evaporation performance, such as Figure 1 As shown, the specific steps are as follows:
[0102] (1) Prepare raw materials:
[0103] Carbon-based nanoparticles: carbon black (manufacturer: Jiaxing Naco New Materials Co., Ltd., brand name: SCC-8-8-1);
[0104] Polymer: polypropylene butadiene copolymer (manufacturer: Aladdin Chemical Reagent Co., Ltd., brand name: P304889);
[0105] Hydrophilic fabric: cotton fabric (manufacturer is Dalian Textile Co., Ltd., weight is 60g / m2 );
[0106] Solvent: chloroform (manufacturer: Aladdin Chemical Reagent Co., Ltd.);
[0107] (2) Preparation of carbon-based nanoparticle / polymer mixed solution:
[0108] (2.1) Add the polymer to the solvent and stir at 30°C for 4 h at a speed of 1000 r / min to obtain a polymer solution; the concentration of the polymer in the polymer solution is 120 g / L;
[0109] (2.2) adding carbon-based nanoparticles to the polymer solution, stirring for 4 hours, and then ultrasonicating for 30 minutes to obtain a carbon-based nanoparticle / polymer mixed solution; the concentration of the carbon-based nanoparticles in the carbon-based nanoparticle / polymer mixed solution is 30 g / L;
[0110] (3) Preparation of composite photothermal fabrics:
[0111] The hydrophilic fabric was ironed and coated with a carbon-based nanoparticle / polymer mixed solution using a scraper, and then quickly placed in a closed environment with a temperature of 25°C and a relative humidity of 99% for 1 hour (water droplet template method) to obtain a composite photothermal fabric with high evaporation performance.
[0112] A composite photothermal fabric with high evaporation performance is prepared by the above method, such as Figure 2 As shown, it is composed of a carbon-based polymer porous membrane and a hydrophilic fabric. The carbon-based polymer porous membrane is mainly composed of a polymer and carbon-based nanoparticles dispersed therein; the thickness of the carbon-based polymer porous membrane is 40 μm, the average pore size is 7 μm, and the porosity is 93%; the thickness of the hydrophilic fabric is 450 μm, the average pore size is 25 μm, and the porosity is 88%;
[0113] The light absorption rate of the composite photothermal fabric is 94.3% and the air permeability is 262mm·s -1 , moisture permeability is 3198g·m -2 ·d -1 The photo-vapor conversion efficiency of pure water is 93.3%, and the water evaporation rate is 1.41 kg·m -2 ·h -1 The light-to-steam conversion efficiency of 3.5 wt% NaCl aqueous solution is 87.5%, and the water evaporation rate is 1.25 kg·m -2 ·h -1 ; The composite photothermal fabric can be recycled 16 times.
[0114] Example 5
[0115] A method for producing a composite photothermal fabric with high evaporation performance, the specific steps are as follows:
[0116] (1) Prepare raw materials:
[0117] Carbon-based nanoparticles: a mixture of carbon black (manufacturer: Jiaxing Naco New Materials Co., Ltd., brand name: SCC-8-8-1) and carbon nanotubes (manufacturer: Shanghai Baiyan Industrial Co., Ltd., brand name: C311) in a mass ratio of 1:1;
[0118] Polymer: polystyrene (manufacturer: Roen Chemical Reagent Co., Ltd., brand: R027658-100g);
[0119] Hydrophilic fabric: cotton fabric (manufacturer: Shanghai Zhongcai Cotton Textile Co., Ltd., weight: 50g / m 2 );
[0120] Solvent: chloroform (manufacturer: Roen Chemical Reagent Co., Ltd.);
[0121] (2) Preparation of carbon-based nanoparticle / polymer mixed solution:
[0122] (2.1) Add the polymer to the solvent and stir at 2000 r / min at 30°C for 5 h to obtain a polymer solution; the concentration of the polymer in the polymer solution is 130 g / L;
[0123] (2.2) adding carbon-based nanoparticles to the polymer solution, stirring for 1 hour, and then ultrasonicating for 30 minutes to obtain a carbon-based nanoparticle / polymer mixed solution; the concentration of the carbon-based nanoparticles in the carbon-based nanoparticle / polymer mixed solution is 40 g / L;
[0124] (3) Preparation of composite photothermal fabrics:
[0125] The hydrophilic fabric was ironed and coated with a carbon-based nanoparticle / polymer mixed solution using a scraper, and then quickly placed in a closed environment with a temperature of 25°C and a relative humidity of 80% for 1 hour (water droplet template method) to obtain a composite photothermal fabric with high evaporation performance.
[0126] A composite photothermal fabric with high evaporation performance prepared by the above method is composed of a carbon-based polymer porous membrane and a hydrophilic fabric. The carbon-based polymer porous membrane is mainly composed of a polymer and carbon-based nanoparticles dispersed therein; the carbon-based polymer porous membrane has a thickness of 50 μm, an average pore size of 6 μm, and a porosity of 85%; the hydrophilic fabric has a thickness of 450 μm, an average pore size of 35 μm, and a porosity of 90%;
[0127] The light absorption rate of the composite photothermal fabric is 95.6%, and the air permeability is 241mm·s -1 , moisture permeability is 3163g·m -2 ·d-1 The light vapor conversion efficiency of pure water is 92.1%, and the water evaporation rate is 1.32 kg·m -2 ·h -1 The light vapor conversion efficiency of 3.5wt% NaCl aqueous solution is 83.3%, and the water evaporation rate is 1.17kg·m -2 ·h -1 ; The composite photothermal fabric can be recycled 18 times.
[0128] Example 6
[0129] A method for producing a composite photothermal fabric with high evaporation performance, the specific steps are as follows:
[0130] (1) Prepare raw materials:
[0131] Carbon-based nanoparticles: redox graphene (manufacturer: Qinghe County Tenghui Metal Materials Co., Ltd., brand name: XF248-7440-44-0);
[0132] Polymer: cellulose acetate (manufacturer: Shanghai Boer Chemical Reagent Co., Ltd., brand number: C804765);
[0133] Hydrophilic fabric: Modal fiber fabric (manufacturer: Tongxiang Allegans Textile Co., Ltd., weight 40g / m 2 );
[0134] Solvent: acetone (manufacturer: Shanghai Boer Chemical Reagent Co., Ltd.);
[0135] (2) Preparation of carbon-based nanoparticle / polymer mixed solution:
[0136] (2.1) Add the polymer to the solvent and stir at 4000 r / min at 50° C. for 2 h to obtain a polymer solution; the concentration of the polymer in the polymer solution is 180 g / L;
[0137] (2.2) adding carbon-based nanoparticles to the polymer solution, stirring for 6 hours, and then ultrasonicating for 40 minutes to obtain a carbon-based nanoparticle / polymer mixed solution; the concentration of the carbon-based nanoparticles in the carbon-based nanoparticle / polymer mixed solution is 45 g / L;
[0138] (3) Preparation of composite photothermal fabrics:
[0139] The hydrophilic fabric was ironed and coated with a carbon-based nanoparticle / polymer mixed solution using a scraper, and then quickly placed in a closed environment with a temperature of 35°C and a relative humidity of 87% for 3.5 hours (water droplet template method) to obtain a composite photothermal fabric with high evaporation performance.
[0140] A composite photothermal fabric with high evaporation performance prepared by the above method is composed of a carbon-based polymer porous membrane and a hydrophilic fabric. The carbon-based polymer porous membrane is mainly composed of a polymer and carbon-based nanoparticles dispersed therein; the carbon-based polymer porous membrane has a thickness of 60 μm, an average pore size of 5 μm, and a porosity of 80%; the hydrophilic fabric has a thickness of 500 μm, an average pore size of 45 μm, and a porosity of 95%;
[0141] The light absorption rate of the composite photothermal fabric is 97.1%, and the air permeability is 231mm·s -1 , moisture permeability is 3065g·m -2 ·d -1 The light vapor conversion efficiency of pure water is 90.3%, and the water evaporation rate is 1.28 kg·m -2 ·h -1 The light vapor conversion efficiency of 3.5wt% NaCl aqueous solution is 87.5%, and the water evaporation rate is 1.11kg·m -2 ·h -1 ; The composite photothermal fabric can be recycled 17 times.
[0142] Example 7
[0143] A method for producing a composite photothermal fabric with high evaporation performance, the specific steps are as follows:
[0144] (1) Prepare raw materials:
[0145] Carbon-based nanoparticles: carbon nanotubes (manufacturer: Jiaxing Naco New Materials Co., Ltd., brand name: SCC-8-8-1);
[0146] Polymer: polyphenylene ether sulfone (manufacturer: Aladdin Chemical Reagent Co., Ltd., brand number: CB5945326);
[0147] Hydrophilic fabric: Lyocell fiber fabric (manufacturer: Jiangsu Carnation Weaving Co., Ltd., weight 70g / m 2 );
[0148] Solvent: toluene (manufacturer: Aladdin Chemical Reagent Co., Ltd.);
[0149] (2) Preparation of carbon-based nanoparticle / polymer mixed solution:
[0150] (2.1) Add the polymer to the solvent and stir at 30°C for 3 h at a speed of 3000 r / min to obtain a polymer solution; the concentration of the polymer in the polymer solution is 200 g / L;
[0151] (2.2) adding carbon-based nanoparticles to the polymer solution, stirring for 2 h, and then ultrasonicating for 60 min to obtain a carbon-based nanoparticle / polymer mixed solution; the concentration of the carbon-based nanoparticles in the carbon-based nanoparticle / polymer mixed solution is 45 g / L;
[0152] (3) Preparation of composite photothermal fabrics:
[0153] The hydrophilic fabric is ironed and coated with a carbon-based nanoparticle / polymer mixed solution using a scraper, and then quickly placed in a closed environment at a temperature of 45°C and a relative humidity of 85% for 4 hours (water droplet template method) to obtain a composite photothermal fabric with high evaporation performance.
[0154] A composite photothermal fabric with high evaporation performance prepared by the above method is composed of a carbon-based polymer porous membrane and a hydrophilic fabric. The carbon-based polymer porous membrane is mainly composed of a polymer and carbon-based nanoparticles dispersed therein; the carbon-based polymer porous membrane has a thickness of 80 μm, an average pore size of 3 μm, and a porosity of 70%; the hydrophilic fabric has a thickness of 600 μm, an average pore size of 10 μm, and a porosity of 80%;
[0155] The light absorption rate of the composite photothermal fabric is 98.6% and the air permeability is 218mm·s -1 , moisture permeability is 3002g·m -2 ·d -1 The light vapor conversion efficiency of pure water is 89.2%, and the water evaporation rate is 1.23 kg·m -2 ·h -1 The light vapor conversion efficiency of 3.5wt% NaCl aqueous solution is 84.6%, and the water evaporation rate is 1.09kg·m -2 ·h -1 ; The composite photothermal fabric can be recycled 16 times.
[0156] Example 8
[0157] A method for producing a composite photothermal fabric with high evaporation performance, the specific steps are as follows:
[0158] (1) Prepare raw materials:
[0159] Carbon-based nanoparticles: a mixture of carbon black (manufacturer: Jiaxing Naco New Materials Co., Ltd., brand name: SCC-8-8-1) and graphene oxide (manufacturer: Qinghe County Tenghui Metal Materials Co., Ltd., brand name: XF248-7440-44-0) in a mass ratio of 1:1;
[0160] Polymer: Hydroxypropyl cellulose (manufacturer: Roen Chemical Reagent Co., Ltd., brand number: SJ00135741395);
[0161] Hydrophilic fabric: Aramid fabric treated with hydrophilic treatment (manufacturer: Dalian Textile Co., Ltd., weight 60g / m 2 );
[0162] Solvent: dimethylformamide (manufacturer: Roen Chemical Reagent Co., Ltd.);
[0163] (2) Preparation of carbon-based nanoparticle / polymer mixed solution:
[0164] (2.1) Add the polymer to the solvent and stir at 40°C for 1 hour at a speed of 5000 r / min to obtain a polymer solution; the concentration of the polymer in the polymer solution is 300 g / L;
[0165] (2.2) adding carbon-based nanoparticles to the polymer solution, stirring for 3 hours, and then ultrasonicating for 50 minutes to obtain a carbon-based nanoparticle / polymer mixed solution; the concentration of the carbon-based nanoparticles in the carbon-based nanoparticle / polymer mixed solution is 50 g / L;
[0166] (3) Preparation of composite photothermal fabrics:
[0167] The hydrophilic fabric was ironed and coated with a carbon-based nanoparticle / polymer mixed solution using a scraper, and then quickly placed in a closed environment with a temperature of 60°C and a relative humidity of 95% for 0.5 h (water droplet template method) to obtain a composite photothermal fabric with high evaporation performance.
[0168] A composite photothermal fabric with high evaporation performance prepared by the above method is composed of a carbon-based polymer porous membrane and a hydrophilic fabric. The carbon-based polymer porous membrane is mainly composed of a polymer and carbon-based nanoparticles dispersed therein; the carbon-based polymer porous membrane has a thickness of 100 μm, an average pore size of 1 μm, and a porosity of 65%; the hydrophilic fabric has a thickness of 600 μm, an average pore size of 15 μm, and a porosity of 83%;
[0169] The light absorption rate of the composite photothermal fabric is 99.5%, and the air permeability is 201mm·s -1 , moisture permeability is 2983g·m -2 ·d -1 The light vapor conversion efficiency of pure water is 85.2%, and the water evaporation rate is 1.12 kg·m -2 ·h -1 The light vapor conversion efficiency of 3.5wt% NaCl aqueous solution is 81.4%, and the water evaporation rate is 1.01kg·m -2 ·h -1 ; The composite photothermal fabric can be recycled 18 times.
Claims
1. A method for preparing a composite photothermal fabric with high evaporation performance, characterized in that: After coating a carbon-based nanoparticle / polymer mixed solution on a hydrophilic fabric, a carbon-based polymer porous membrane is formed by a water drop template method, thereby obtaining a composite photothermal fabric with high evaporation performance, wherein the carbon-based nanoparticle / polymer mixed solution mainly consists of carbon-based nanoparticles, polymers and solvents; The composite photothermal fabric with high evaporation performance includes a carbon-based polymer porous membrane and a hydrophilic fabric adjacent thereto; The carbon-based polymer porous membrane is mainly composed of a polymer and carbon-based nanoparticles dispersed therein; the thickness of the carbon-based polymer porous membrane is 10 to 100 μm, the average pore size is 1 to 10 μm, and the porosity is 65% to 95%; The polymer is a hydrophilic polymer or a hydrophobic polymer; The thickness of the hydrophilic fabric is 400-600 μm; the hydrophilic fabric is cotton fabric, spandex fabric, viscose fiber fabric, modal fiber fabric, lyocell fiber fabric, bamboo fiber fabric, wool fabric, hydrophilized polyester fabric, hydrophilized acrylic fabric, hydrophilized nylon fabric, hydrophilized aramid fabric or hydrophilized carbon fiber fabric.
2. The method for preparing a composite photothermal fabric with high evaporation performance according to claim 1, characterized in that: The preparation process of carbon-based nanoparticle / polymer mixed solution is as follows: (1) adding the polymer to the solvent, stirring at a speed of 1000 to 5000 r / min at 30 to 50° C. for 1 to 5 hours, to obtain a polymer solution; the concentration of the polymer in the polymer solution is 50 to 300 g / L; (2) Adding carbon-based nanoparticles to the polymer solution, stirring for 1 to 6 hours, and then ultrasonicating for 10 to 60 minutes to obtain a carbon-based nanoparticle / polymer mixed solution; the concentration of the carbon-based nanoparticles in the carbon-based nanoparticle / polymer mixed solution is 5 to 50 g / L.
3. The method for preparing a composite photothermal fabric with high evaporation performance according to claim 1, characterized in that: The specific process is: iron the hydrophilic fabric, coat its surface with a carbon-based nanoparticle / polymer mixed solution with a scraper, and then quickly place it in a closed environment with a temperature of 20-60°C and a relative humidity of 65%-99% and let it stand for 0.5-5 hours to obtain a composite photothermal fabric with high evaporation performance.
4. The method for preparing a composite photothermal fabric with high evaporation performance according to claim 1, characterized in that: The light absorption rate of the composite photothermal fabric is above 90%, and the air permeability is 201-291 mm·s -1 , moisture permeability is 2983~3392g·m -2 ·d -1 ; The photothermal conversion efficiency of the composite photothermal fabric to pure water is 85.2% to 98.2%, and the water evaporation rate is 1.12 to 1.41 kg·m -2 ·h -1 ; The photothermal conversion efficiency of the composite photothermal fabric for 3.5wt% NaCl aqueous solution is 81.4% to 92.1%, and the water evaporation rate is 1.01 to 1.37 kg·m -2 ·h -1 ; The composite photothermal fabric can be recycled for no less than 15 times.
5. The method for preparing a composite photothermal fabric with high evaporation performance according to claim 1, characterized in that: The average pore size of the hydrophilic fabric is larger than that of the carbon-based polymer porous membrane; the average pore size of the hydrophilic fabric is 10-50 μm, and the porosity is 80%-99%.
6. The method for preparing a composite photothermal fabric with high evaporation performance according to claim 1, characterized in that: The carbon-based nanoparticles are one or more of carbon black, graphene oxide, redox graphene and carbon nanotubes.
7. The method for preparing a composite photothermal fabric with high evaporation performance according to claim 1, characterized in that: The polymer is one or more of polypropylene butadiene copolymer, polydimethylsiloxane, polystyrene, polysulfone resin, polyphenylene ether sulfone, polyetherimide, cellulose acetate, methyl cellulose, carboxymethyl cellulose, ethyl cellulose, hydroxyethyl cellulose, cyanoethyl cellulose, hydroxypropyl cellulose and hydroxypropyl methyl cellulose.
8. The method for preparing a composite photothermal fabric with high evaporation performance according to claim 7, characterized in that: The polymer is polypropylene butadiene copolymer, and the hydrophilic fabric is cotton fabric; or, the polymer is polystyrene, and the hydrophilic fabric is cotton fabric; or, the polymer is cellulose acetate, and the hydrophilic fabric is modal fiber fabric; or, the polymer is polyphenylene ether sulfone, and the hydrophilic fabric is lyocell fiber fabric; or, the polymer is hydroxypropyl cellulose, and the hydrophilic fabric is aramid fabric after hydrophilization treatment.